Degradable hot melt adhesive and preparation process thereof
Through the blending of ethylene-vinyl acetate copolymer and polylactic acid and the coordination of nanofillers, the problems of poor biodegradation and deterioration of EVA hot melt adhesives are solved, and efficient biodegradation and bonding performance are achieved. .
Patent Information
- Application Number
- CN202411179512.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The biodegradable properties of EVA-type hot melt adhesives are poor, and simple mixing of degradable hot melt resins can easily lead to a decrease in bonding performance, making it difficult to take into account both.
Ethylene-vinyl acetate copolymer is used to blend with polylactic acid, and compatibility and crystallinity are improved through nanofillers (sheet nanoboehmite and spherical nanoalumina), thereby improving bonding and biodegradation performance.
It effectively improves the biodegradation performance and bonding strength of hot melt adhesives, avoids bonding failure, and achieves efficient bonding performance and biodegradation through uniform mixing and crystallization promotion.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polymer materials and more specifically relates to a degradable hot melt adhesive and a preparation process thereof. Background Art
[0002] Hot melt adhesive is mainly used for wood or paper composite packaging or binding, and is also used for rapid bonding in industries such as automobiles, ships, and building interior decoration.
[0003] Hot melt adhesive is a thermoplastic material made by melting thermoplastic resin as the matrix and supplemented with tackifiers, plasticizers, antioxidants and other ingredients. It has become a commonly used adhesive in various industries in modern society due to its excellent performance and convenient application. At present, the hot melt adhesive market at home and abroad is mostly dominated by EVA hot melt adhesive, which also includes different product types such as polyethylene, polypropylene, polyamide, polyimide, polyester, polyurethane, etc. The matrix resins are all high molecular organic matter with special chemical structures and characteristics that are difficult to biodegrade. With the widespread and in-depth application of hot melt adhesives, they have been retained in the environment for a long time and have become hidden dangers and hazards to the ecological environment. Therefore, under the situation of global ecological protection and sustainable development, research on new green and environmentally friendly biodegradable hot melt adhesives has become an important development direction for the adhesive industry today.
[0004] When recycling products bonded with hot melt adhesives, the hot melt adhesives must be biodegradable or chemically degradable, otherwise it will be extremely difficult to recycle. Of course, while improving the environmental friendliness of hot melt adhesives, it is also necessary to improve the bonding properties of hot melt adhesives. Summary of the invention
[0005] The technical problem to be solved by the present invention is: for EVA hot melt adhesives, their biodegradability is poor, and simply mixing in degradable hot melt resins easily leads to the problem that the bonding properties of the hot melt adhesive itself cannot be effectively taken into account. The present invention provides a degradable hot melt adhesive and a preparation process thereof.
[0006] The purpose of the invention is to provide a degradable hot melt adhesive.
[0007] Another object of the present invention is to provide a process for preparing a degradable hot melt adhesive.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A degradable hot melt adhesive comprises the following raw materials in parts by weight:
[0010] 90-100 parts of ethylene-vinyl acetate copolymer, 18-20 parts of polylactic acid, 8-10 parts of nanofiller, 1-3 parts of plasticizer, 1-3 parts of antioxidant, 2-4 parts of microcrystalline wax;
[0011] Wherein, the nano filler is composed of flaky nano boehmite and spherical nano alumina in a mass ratio of (0.9-1.0):1;
[0012] The D50 of the flaky nano-boehmite is 65-70 nm;
[0013] The D50 of the spherical nano-alumina is 10-15 nm.
[0014] Beneficial effects of the above scheme:
[0015] By using the ethylene-vinyl acetate copolymer and polylactic acid blend system as the main components of the hot melt adhesive, firstly, polylactic acid has good biodegradability. After adding polylactic acid, the biodegradability of ethylene-vinyl acetate copolymer alone as the main component of the hot melt adhesive can be improved; secondly, polylactic acid contains a large number of ester groups in its molecular structure. The introduction of ester groups can increase the interfacial force of the hot melt adhesive system on the substrate, thereby improving the bonding strength of the product; in addition, polylactic acid itself is a semi-crystalline polymer. By adjusting the amount of addition, the crystallization behavior of ethylene-vinyl acetate copolymer can be affected. Specifically, the crystallinity of the hot melt adhesive system can be improved, thereby further improving the reliability of product bonding and avoiding the bonding failure caused by excessive erosion by oxygen and water in the air during normal use;
[0016] However, the inventors found that when ethylene-vinyl acetate copolymer and polylactic acid are blended, due to their different chemical structures and polarities, there are compatibility problems between the two, making it difficult to mix the two evenly using conventional methods. If the melt mixing is carried out for too long during the preparation process, it is easy to cause oxidation of the hot melt adhesive. The inventors found that this problem can be significantly improved by adding a nanofiller system composed of flaky nano-boehmite and spherical nano-alumina. Specifically, the combination of two nanofillers with different morphologies can work together as a stress transfer medium during the resin blending process to improve the overall stress transfer efficiency, thereby accelerating the mixing between the two different resins. In addition, the two can act as nucleating agents to promote the crystallization of the resin, increase the crystallization rate and crystallinity, and thus improve the bonding performance. In addition, thanks to the good water absorption performance of boehmite, it can improve the biodegradability of the product in the later stage of use.
[0017] Furthermore, the particle size distribution range of the flaky nano-boehmite is 30-90 nm; and the particle size distribution range of the spherical nano-alumina is 1-30 nm.
[0018] Furthermore, the sphericity of the spherical nano-alumina is 8.8-9.2.
[0019] Furthermore, the surfaces of the flaky nano-boehmite and the spherical nano-alumina are coated with a silane coupling agent;
[0020] The silane coupling agent is selected from any one of silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570.
[0021] Furthermore, the weight average molecular weight Mw of the polylactic acid is 20000-30000 g / mol.
[0022] Furthermore, the plasticizer is selected from any one of tributyl citrate, acetyl tributyl citrate, epoxy soybean oil, dicyclohexyl phthalate, glycerol tribenzoate or trimethylolpropane tribenzoate.
[0023] Furthermore, the antioxidant is selected from any one of antioxidant 801, butylated hydroxytoluene, thiobis(3-methyl-6-tert-butyl)phenol, and 2,6-di-tert-butyl-p-cresol.
[0024] A method for preparing a degradable hot melt adhesive, the specific preparation steps comprising:
[0025] Weigh each component according to the raw material composition;
[0026] First, ethylene-vinyl acetate copolymer, polylactic acid, plasticizer, antioxidant, microcrystalline wax and spherical nano-alumina are mixed, heated to 150-155° C., and stirred for premixing;
[0027] After the stirring and premixing is completed, add the flaky nano-boehmite, heat to 160-165°C, and then stir and final mix;
[0028] Cooling and solidification, discharging, and obtaining the degradable hot melt adhesive.
[0029] Beneficial effects of the above scheme:
[0030] During the melt blending process, spherical nano-alumina is first added. At the initial stage of stirring shear force, under the condition of relatively low temperature, the system viscosity is relatively large, and the shear force is relatively large. Under the action of spherical nano-alumina, the molecular chains of two different resins are fully stretched in the initial stage of mixing shear, thereby achieving sufficient preliminary dispersion. Then, under the condition of higher temperature, flaky nano-boehmite is added. Under this condition, the polylactic acid resin is fully melted and the system viscosity begins to decrease, which is conducive to the rapid and uniform dispersion of the flaky boehmite. Through the two-step mixing, both the uniform mixing of the components can be achieved and the oxidation decomposition of the resin caused by too long mixing can be avoided.
[0031] Furthermore,
[0032] The stirring premixing comprises: stirring and mixing for 25-30 minutes at a rotation speed of 180-200 r / min;
[0033] The stirring and final mixing comprises: stirring and mixing for 45-60 minutes at a rotation speed of 320-350 r / min.
[0034] Furthermore, the cooling and solidification includes: cooling to room temperature at a cooling rate of 2.0-2.5°C / min.
[0035] By further controlling the cooling and solidification rate, the crystallization rate of the resin under the action of the nano-seasoning can be regulated. DETAILED DESCRIPTION
[0036] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0037] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0038] Example 1
[0039] According to weight, 90 parts of ethylene-vinyl acetate copolymer, 18 parts of polylactic acid, 8 parts of nanofiller, 1 part of plasticizer, 1 part of antioxidant, and 2 parts of microcrystalline wax are taken in sequence;
[0040] Wherein, the nano filler is composed of flaky nano boehmite and spherical nano alumina in a mass ratio of 0.9:1;
[0041] The D50 of the flaky nano-boehmite is 65 nm;
[0042] The D50 of the spherical nano-alumina is 10 nm;
[0043] The particle size distribution range of the flaky nano-boehmite is 30-90 nm; and the particle size distribution range of the spherical nano-alumina is 1-30 nm;
[0044] The sphericity of the spherical nano-alumina is 8.8;
[0045] The surfaces of the flaky nano-boehmite and the spherical nano-alumina are coated with a silane coupling agent;
[0046] The silane coupling agent is selected from silane coupling agent KH-550;
[0047] The weight average molecular weight Mw of the polylactic acid is 20000 g / mol;
[0048] The plasticizer is selected from tributyl citrate;
[0049] The antioxidant is selected from antioxidant 801;
[0050] First, ethylene-vinyl acetate copolymer, polylactic acid, plasticizer, antioxidant, microcrystalline wax and spherical nano-alumina are mixed, heated to 150° C., and stirred and pre-mixed for 25 minutes at a rotation speed of 180 r / min to obtain a premix;
[0051] Adding flaky nano-boehmite to the premix, heating to 160° C., stirring and mixing at a speed of 320 r / min for 45 minutes to obtain a final mixture;
[0052] The final mixture was cooled to room temperature at a cooling rate of 2.0° C. / min to solidify the final mixture, thereby obtaining a degradable hot melt adhesive.
[0053] Example 2
[0054] According to weight, 95 parts of ethylene-vinyl acetate copolymer, 19 parts of polylactic acid, 9 parts of nanofiller, 2 parts of plasticizer, 2 parts of antioxidant, and 3 parts of microcrystalline wax are taken in sequence;
[0055] Wherein, the nano filler is composed of flaky nano boehmite and spherical nano alumina in a mass ratio of 0.96:1;
[0056] The D50 of the flaky nano-boehmite is 68 nm;
[0057] The D50 of the spherical nano-alumina is 12 nm;
[0058] The particle size distribution range of the flaky nano-boehmite is 30-90 nm; and the particle size distribution range of the spherical nano-alumina is 1-30 nm;
[0059] The sphericity of the spherical nano-alumina is 9;
[0060] The surfaces of the flaky nano-boehmite and the spherical nano-alumina are coated with a silane coupling agent;
[0061] The silane coupling agent is selected from silane coupling agent KH-560;
[0062] The weight average molecular weight Mw of the polylactic acid is 25000 g / mol;
[0063] The plasticizer is selected from acetyl tributyl citrate;
[0064] The antioxidant is selected from butylated hydroxytoluene;
[0065] First, ethylene-vinyl acetate copolymer, polylactic acid, plasticizer, antioxidant, microcrystalline wax and spherical nano-alumina are mixed, heated to 152° C., and stirred and pre-mixed for 28 minutes at a rotation speed of 190 r / min to obtain a premix;
[0066] Adding flaky nano-boehmite to the premix, heating to 163° C., stirring and mixing at a rotation speed of 330 r / min for 50 min to obtain a final mixture;
[0067] The final mixture was cooled to room temperature at a cooling rate of 2.2° C. / min to solidify the final mixture, thereby obtaining a degradable hot melt adhesive.
[0068] Example 3
[0069] According to weight, 100 parts of ethylene-vinyl acetate copolymer, 20 parts of polylactic acid, 10 parts of nanofiller, 3 parts of plasticizer, 3 parts of antioxidant, and 4 parts of microcrystalline wax are taken in sequence;
[0070] Wherein, the nano filler is composed of flaky nano boehmite and spherical nano alumina in a mass ratio of 1:1;
[0071] The D50 of the flaky nano-boehmite is 70 nm;
[0072] The D50 of the spherical nano-alumina is 15 nm;
[0073] The particle size distribution range of the flaky nano-boehmite is 30-90 nm; and the particle size distribution range of the spherical nano-alumina is 1-30 nm;
[0074] The sphericity of the spherical nano-alumina is 9.2;
[0075] The surfaces of the flaky nano-boehmite and the spherical nano-alumina are coated with a silane coupling agent;
[0076] The silane coupling agent is selected from silane coupling agent KH-570;
[0077] The weight average molecular weight Mw of the polylactic acid is 30000 g / mol;
[0078] The plasticizer is selected from epoxidized soybean oil;
[0079] The antioxidant is selected from thiobis(3-methyl-6-tert-butyl)phenol;
[0080] First, ethylene-vinyl acetate copolymer, polylactic acid, plasticizer, antioxidant, microcrystalline wax and spherical nano-alumina are mixed, heated to 155° C., and stirred and pre-mixed for 30 minutes at a rotation speed of 200 r / min to obtain a premix;
[0081] Adding flaky nano-boehmite to the premix, heating to 165° C., stirring and mixing at a speed of 350 r / min for 60 min to obtain a final mixture;
[0082] The final mixture was cooled to room temperature at a cooling rate of 2.5° C. / min to solidify the final mixture, thereby obtaining a degradable hot melt adhesive.
[0083] Example 4
[0084] Compared with Example 1, this embodiment is different in that:
[0085] The particle size distribution range of the flaky nano-boehmite is 10-120 nm; and the particle size distribution range of the spherical nano-alumina is 0.1-60 nm; the other conditions remain unchanged.
[0086] Example 5
[0087] Compared with Example 1, this embodiment is different in that:
[0088] The sphericity of the spherical nano-alumina is 8.4, and other conditions remain unchanged.
[0089] Example 6
[0090] Compared with Example 1, this embodiment is different in that:
[0091] First, ethylene-vinyl acetate copolymer, polylactic acid, plasticizer, antioxidant, microcrystalline wax and flaky nano-boehmite are mixed, heated to 150° C., and stirred and pre-mixed for 25 minutes at a rotation speed of 180 r / min to obtain a premix;
[0092] Then, spherical nano-alumina was added to the premix, heated to 160° C., and stirred and mixed for 45 minutes at a rotation speed of 320 r / min to obtain a final mixture;
[0093] The rest of the conditions remain unchanged.
[0094] Comparative Example 1
[0095] The difference between this comparative example and Example 1 is that no flaky nano-boehmite is added, and other conditions remain unchanged.
[0096] Comparative Example 2
[0097] The difference between this comparative example and Example 1 is that no spherical nano-alumina is added, and the other conditions remain unchanged.
[0098] Comparative Example 3
[0099] The difference between this comparative example and Example 1 is that polylactic acid is not added, and the other conditions remain unchanged.
[0100] The performance tests were performed on the products obtained in the above examples and comparative examples. The specific test methods and test results are as follows:
[0101] Tensile strength test:
[0102] According to GB / T528-1998 test standard, test conditions: electronic tensile testing machine, temperature 25℃, humidity 50%, tensile rate 50mm / min, test 5 samples and take the average value; detailed test results are shown in Table 1;
[0103] Biodegradation performance test:
[0104] Using the soil burial method, a 10cm×10cm square thin film weighed m1 was buried in moist soil, taken out after one month, dried and weighed m2, and its degradation performance was characterized by its mass change rate. The detailed test results are shown in Table 1;
[0105] Mass change rate = (m1-m2) / m1×100%;
[0106] Table 1: Product performance test results:
[0107] Tensile strength / MPa Quality change rate / % Example 1 5.28 27.6 Example 2 5.35 28.2 Example 3 5.44 28.3 Example 4 5.11 26.6 Example 5 5.14 26.8 Example 6 5.08 26.3 Comparative Example 1 4.55 23.5 Comparative Example 2 4.63 24.1 Comparative Example 3 4.44 18.5
[0108] It can be seen from the test results in Table 1 that the product obtained by the present invention can effectively guarantee the basic bonding performance of the product and also have higher biodegradability.
[0109] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A degradable hot melt adhesive, characterized in that: The invention comprises the following raw materials in parts by weight: 90-100 parts of ethylene-vinyl acetate copolymer, 18-20 parts of polylactic acid, 8-10 parts of nanofiller, 1-3 parts of plasticizer, 1-3 parts of antioxidant, 2-4 parts of microcrystalline wax; Wherein, the nano filler is composed of flaky nano boehmite and spherical nano alumina in a mass ratio of (0.9-1.0):1; The D50 of the flaky nano-boehmite is 65-70 nm; The D50 of the spherical nano-alumina is 10-15 nm.
2. A degradable hot melt adhesive according to claim 1, characterized in that: The particle size distribution range of the flaky nano-boehmite is 30-90 nm; and the particle size distribution range of the spherical nano-alumina is 1-30 nm.
3. A degradable hot melt adhesive according to any one of claims 1-2, characterized in that: The sphericity of the spherical nano-alumina is 8.8-9.
2.
4. The degradable hot melt adhesive according to claim 1, characterized in that: The surfaces of the flaky nano-boehmite and the spherical nano-alumina are coated with a silane coupling agent; The silane coupling agent is selected from any one of silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570.
5. The degradable hot melt adhesive according to claim 1, characterized in that: The weight average molecular weight Mw of the polylactic acid is 20000-30000 g / mol.
6. The degradable hot melt adhesive according to claim 1, characterized in that: The plasticizer is selected from any one of tributyl citrate, acetyl tributyl citrate, epoxy soybean oil, dicyclohexyl phthalate, glycerol tribenzoate or trimethylolpropane tribenzoate.
7. The degradable hot melt adhesive according to claim 1, characterized in that: The antioxidant is selected from any one of antioxidant 801, butylated hydroxytoluene, thiobis(3-methyl-6-tert-butyl)phenol, and 2,6-di-tert-butyl-p-cresol.
8. A method for preparing the degradable hot melt adhesive according to any one of claims 1 to 7, characterized in that: The specific preparation steps include: Weigh each component according to the raw material composition; First, ethylene-vinyl acetate copolymer, polylactic acid, plasticizer, antioxidant, microcrystalline wax and spherical nano-alumina are mixed, heated to 150-155° C., and stirred for premixing; After the stirring and premixing is completed, add the flaky nano-boehmite, heat to 160-165°C, and then stir and final mix; Cooling and solidification, discharging, and obtaining the degradable hot melt adhesive.
9. The method for preparing a degradable hot melt adhesive according to claim 8, characterized in that: The stirring premixing comprises: stirring and mixing for 25-30 minutes at a rotation speed of 180-200 r / min; The stirring and final mixing comprises: stirring and mixing for 45-60 minutes at a rotation speed of 320-350 r / min.
10. The method for preparing a degradable hot melt adhesive according to claim 8, characterized in that: The cooling and solidification comprises: cooling down to room temperature at a cooling rate of 2.0-2.5°C / min.
Citation Information
Patent Citations
Flame retardant high -strength olefin polymer compsns - - contg hydrated alumina filler including small amt of sodium
CH579119A5
Hot melt adhesive film for compounding metal and PVC (polyvinyl chloride) plastic and preparation method of hot melt adhesive film
CN116120841A
High-voltage quick-charge type lithium ion battery and electrolyte
CN118136945A
Hot melt adhesive compositions and use thereof
US20170174958A1