Binder, positive plate, negative plate, battery, battery pack and electric equipment
By using modified nitrile rubber and low crystallinity polyvinylidene fluoride polymer binder in lithium battery pole sheets, the problems of improving flexibility and decreasing energy density of lithium battery pole sheets are solved, and high energy is achieved Density and long cycle life battery performance.
Patent Information
- Application Number
- CN202411506687.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When improving flexibility, existing lithium battery electrodes often need to reduce surface density and compaction density, resulting in a decrease in battery volume energy density, which violates the design rules of lithium battery products.
Adopt a binder containing modified nitrile rubber and a polyvinylidene fluoride polymer with a certain calorific value enthalpy, thereby improving the flexibility of the electrode sheet through its alkyl chain structure and low crystallinity, avoiding reducing the electrode sheet density and compaction Density, thereby increasing the volume energy density of the battery.
Without reducing the surface density and compaction density of the electrode sheet, the flexibility of the electrode sheet is significantly improved, the cycle life of the battery is extended, and the energy density is improved, achieving the effect of high energy density and long cycle life.
Smart Images

Figure CN119019956A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of batteries, and in particular to a binder, a positive electrode sheet, a negative electrode sheet, a battery, a battery pack and electrical equipment. Background Art
[0002] Electrode sheets with good flexibility can better adapt to volume changes during the charge and discharge cycle, reduce the powdering and shedding of electrode materials, thereby helping to extend the cycle life of the battery. In addition, electrode sheets with good flexibility can be wound or stacked more tightly, thereby increasing the energy density of the battery.
[0003] At present, the flexibility of lithium battery pole pieces is mainly improved from the following two aspects: reducing the compaction density and reducing the surface density. However, both the reduction of surface density and the reduction of compaction will reduce the amount of active materials per unit volume, resulting in a decrease in the volume energy density of the battery, which does not conform to the design rules of lithium battery products. Summary of the invention
[0004] The present invention provides an adhesive which can improve the flexibility of a pole piece without reducing the surface density and compaction of the pole piece.
[0005] The present invention also provides a positive electrode sheet. Since the positive electrode sheet includes the above-mentioned binder, compared with the traditional positive electrode sheet, it can have good flexibility without reducing the surface density and compaction, thereby helping to improve the volume energy density of the battery.
[0006] The present invention also provides a negative electrode sheet. Since the negative electrode sheet includes the above-mentioned binder, compared with the traditional negative electrode sheet, it can have good flexibility without reducing the surface density and compaction, thereby helping to improve the volume energy density of the battery.
[0007] The present invention also provides a battery. Since the battery includes the positive electrode sheet and / or the negative electrode sheet, the battery has a longer cycle life and a higher energy density.
[0008] The present invention also provides a battery pack. Since the battery pack includes the above-mentioned battery, the battery pack has the advantages of high energy density, long cycle life and good rate performance.
[0009] The present invention also provides an electrical device. Since the electrical device comprises the battery or battery pack, the electrical device has good electrical performance and a long service life.
[0010] In detail, in a first aspect, the present invention provides a binder, comprising a modified nitrile rubber and / or a polyvinylidene fluoride-based polymer; the modified nitrile rubber comprises a structure shown in Formula 1 and / or Formula 2: Formula 1, Formula 2, In Formula 1, R1 and R3 are each independently an alkyl chain greater than or equal to C8, R2 is an alkyl chain greater than or equal to C6, and x is greater than or equal to 1; In Formula 2, R4 and R6 are each independently an alkyl chain of C8 or greater, R5 is an alkyl chain of C6 or greater, and x is greater than or equal to 1; The calorific value enthalpy of the polyvinylidene fluoride-based polymer is less than or equal to 30 J / g.
[0011] Furthermore, in Formula 1, R1 and R3 are each independently a branched alkyl chain of C8-C60 or a branched alkyl chain, and R2 is a branched alkyl chain of C6-C30 or a branched alkyl chain; in Formula 2, R4 and R6 are each independently a branched alkyl chain of C8-C60 or a branched alkyl chain, and R5 is a branched alkyl chain of C6-C30 or a branched alkyl chain.
[0012] Furthermore, the calorific value enthalpy of the polyvinylidene fluoride-based polymer is greater than or equal to 15 J / g.
[0013] Furthermore, the polyvinylidene fluoride based polymer is selected from a mixture of polyvinylidene fluoride and a second polymer, and the second polymer is at least one of polyethylene glycol, polymethyl methacrylate, and polyvinyl acetate; And / or, the polyvinylidene fluoride-based polymer is selected from a copolymer of vinylidene fluoride and a second monomer, and the second monomer is vinyl carboxylate, ethylene glycol oxalate or ethylene glycol succinate.
[0014] Further, the molar content of acrylonitrile in the modified nitrile rubber is 30%-40%; And / or, the molecular weight of the modified nitrile rubber is 200000 g / mol-300000 g / mol; And / or, the degree of hydrogenation of the modified nitrile rubber is 90%-99%.
[0015] In a second aspect, the present invention provides a positive electrode sheet, comprising the binder described in the first aspect, a positive electrode active material and a conductive agent.
[0016] Furthermore, the polyvinylidene fluoride based polymer accounts for 3% to 3.5% of the mass of the positive electrode active material; And / or, the modified nitrile rubber accounts for 0.3%-0.6% of the mass of the positive electrode active material.
[0017] Furthermore, the conductive agent includes carbon nanotubes and conductive carbon black; wherein the D50 of the conductive carbon black is 10nm-100nm; the diameter of the carbon nanotubes is 10nm-150nm, and the specific surface area is 10m2 / g-300m 2 / g.
[0018] Furthermore, the D of the positive electrode active material 50 It is 0.30μm-0.40μm.
[0019] Furthermore, the surface density of the positive electrode sheet is 500g / m 2 -550g / m 2 ; compacted density is 2.45 g / cm 3 -2.55g / cm 3 .
[0020] In a third aspect, the present invention provides a negative electrode sheet, comprising the binder and negative electrode active material described in the first aspect.
[0021] In a fourth aspect, the present invention provides a battery, comprising the positive electrode sheet described in the second aspect, and / or the negative electrode sheet described in the third aspect.
[0022] In a fifth aspect, the present invention provides a battery pack comprising the battery described in the fourth aspect.
[0023] In a sixth aspect, the present invention provides an electrical device, comprising the battery described in the fourth aspect or the battery pack described in the fifth aspect.
[0024] The binder provided by the present invention can improve the flexibility of the pole piece without reducing the pole piece surface density and compaction by adding modified nitrile rubber containing an alkyl chain structure of a certain length and / or a polyvinylidene fluoride based polymer with a certain calorific value enthalpy. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0026] Figure 1 This is a physical picture of the positive electrode sheet of comparative example 1 of the present invention, during the bending resistance test, about 10-15 times; Figure 2 This is a physical picture of the positive electrode sheet of Example 1 of the present invention, which is subjected to a bending resistance test for more than 100 times; Figure 3 This is a scanning calorimetric analysis result diagram of the polyvinylidene fluoride based polymer of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below. The specific implementation methods listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
[0028] In the present invention, the term "glass transition temperature": abbreviated as Tg, refers to the temperature corresponding to the transition of an amorphous polymer material from a glassy state to a highly elastic state.
[0029] In the present invention, the term "crystallinity" is used to indicate the proportion of crystalline regions in a polymer, reflecting the degree of crystallinity within the material.
[0030] In a first aspect, the present invention provides a binder comprising a modified nitrile rubber and / or a polyvinylidene fluoride based polymer; the modified nitrile rubber comprises a structure shown in Formula 1 and / or Formula 2: Formula 1, Formula 2, In Formula 1, R1 and R3 are each independently an alkyl chain greater than or equal to C8, R2 is an alkyl chain greater than or equal to C6, and x is greater than or equal to 1; In Formula 2, R4 and R6 are each independently an alkyl chain of C8 or greater, R5 is an alkyl chain of C6 or greater, and x is greater than or equal to 1; The calorific value enthalpy of the polyvinylidene fluoride-based polymer is less than or equal to 30 J / g.
[0031] The binder provided by the present invention can improve the flexibility of the pole piece without reducing the surface density and compaction of the pole piece. The reasons include: since the modified nitrile rubber contains an alkyl chain structure of a certain length, the modified nitrile rubber with a certain alkyl chain structure has good flexibility and can act as a softener when used for the pole piece, thereby effectively improving the flexibility of the pole piece; and / or, the polyvinylidene fluoride based polymer with a certain calorific value enthalpy has a low crystallinity. Compared with the conventional binder polyvinylidene fluoride, the crystallinity can be reduced by about 15-25%. The lower the crystallinity, the lower its glass transition temperature, and the easier it is to change the molecular arrangement structure, so the flexibility of the pole piece is better.
[0032] In some embodiments, the above-mentioned modified nitrile rubber and a polyvinylidene fluoride-based polymer with a certain calorific value enthalpy are used in combination. The modified nitrile rubber can reduce the excessive entanglement between the CF bonds in polyvinylidene fluoride, thereby weakening the excessive entanglement force between the polyvinylidene fluoride molecular chain and the positive / negative electrode active material particles, thereby further improving the flexibility of the electrode.
[0033] In other embodiments, the modified nitrile rubber may also be used in combination with other conventional adhesives, for example, in combination with conventional polyvinylidene fluoride.
[0034] Illustratively, in Formula 1, R1 and R3 are each independently a branched alkyl chain of C8-C60 or a branched alkyl chain, and R2 is a branched alkyl chain of C6-C30 or a branched alkyl chain; in Formula 2, R4 and R6 are each independently a branched alkyl chain of C8-C60 or a branched alkyl chain, and R5 is a branched alkyl chain of C6-C30 or a branched alkyl chain.
[0035] Furthermore, R1 and R3 are each independently a branched alkyl chain of C10-C20 or an alkyl chain with a branch, R2 is a branched alkyl chain of C10-C20 or an alkyl chain with a branch; R4 and R6 are each independently a branched alkyl chain of C10-C20 or an alkyl chain with a branch, and R5 is a branched alkyl chain of C10-C20 or a alkyl chain with a branch.
[0036] Illustratively, in Formula 1, x is in any range of 1-100, 1-80, 10-80, 10-70, 10-60, 10-50, 10-40, 10-30, 10-20, etc.; in Formula 2, x is in any range of 1-100, 1-80, 10-80, 10-70, 10-60, 10-50, 10-40, 10-30, 10-20, etc.
[0037] In one embodiment, the binder of the present invention can achieve a positive electrode sheet density of 530 g / m 2 -550g / m 2 The compacted density is between 2.50-2.55g / cm 3 Under the design system within the range, the positive electrode sheet will not break or fall off during the winding process, ultimately realizing the feasibility of the winding process under high surface density and high compaction.
[0038] In an optional embodiment, the calorific value enthalpy of the polyvinylidene fluoride based polymer is not less than 15 J / g. The polyvinylidene fluoride based polymer with this calorific value enthalpy has the ability of lower crystallinity, lower glass transition temperature, and easy change of molecular arrangement structure, so the flexibility of the pole piece is better.
[0039] The binder of the above embodiment may be understood as a binder composition including a polyvinylidene fluoride-based polymer and a modified nitrile rubber.
[0040] For example, the calorific value enthalpy of the polyvinylidene fluoride-based polymer can be known by differential scanning calorimetry analysis.
[0041] In a specific embodiment, the polyvinylidene fluoride-based polymer is selected from a mixture of polyvinylidene fluoride and a second polymer, and the second polymer is at least one of polyethylene glycol (PEG), polymethyl methacrylate (PMMA), and polyvinyl acetate (PVAc); And / or, the polyvinylidene fluoride-based polymer is selected from a copolymer of vinylidene fluoride and a second monomer, and the second monomer is vinyl carboxylate, ethylene glycol oxalate or ethylene glycol succinate.
[0042] The copolymer of vinylidene fluoride and the second monomer can be prepared by existing processes, and in some embodiments, a suspension polymerization method is used, which specifically includes the following steps: Taking the monomer vinyl carboxylate as an example, a certain amount of deionized water and dispersant are added to a stainless steel autoclave equipped with a stirring element, the stainless steel autoclave is sealed, evacuated, filled with nitrogen to replace oxygen, stirred, and heated to 50°C at the same time. Vinylidene fluoride (VDF) is filled to make the autoclave pressure reach 3.5MPa, and initiators are added to start the polymerization reaction; continue to add the monomer vinyl carboxylate and the relative proportion of initiators and auxiliary agents at a certain rate, maintain the temperature and pressure; until the monomer is added, the pressure drops to 2.8MPa, stop stirring, the polymerization reaction ends, and collect the sample by centrifugal drying and other methods. When the above-mentioned monomer vinyl carboxylate is replaced by any monomer such as ethylene glycol oxalate and ethylene glycol succinate, its synthesis process can refer to this preparation.
[0043] The initiator may be isopropyl peroxycarbonate (IPP), di(2-ethylhexyl) peroxydicarbonate (EHP), etc.; the dispersant may be a cellulose suspending agent, etc.
[0044] In an optional embodiment, the molar content of acrylonitrile in the modified nitrile rubber is 30%-40%; And / or, the molecular weight of the modified nitrile rubber is 200000 g / mol-300000 g / mol; And / or, the degree of hydrogenation of the modified nitrile rubber is 90%-99%.
[0045] Among them, the mass content of acrylonitrile in the modified nitrile rubber within the above-mentioned range can give the binder better flexibility and ensure high stability of the electrode. If the mass content of acrylonitrile is less than 3 wt%, the solvation ability of the binder may be weakened, thereby affecting the dispersibility of the active particles of the electrode and the structural stability of the electrode. If the mass content of acrylonitrile is greater than 40 wt%, the glass transition temperature of the modified nitrile rubber will be higher, which will affect the flexibility of the binder. In addition, the molecular weight and degree of hydrogenation of the modified nitrile rubber can jointly affect the dispersion effect and softening effect of the modified nitrile rubber with the length of the alkyl chain. The modified nitrile rubber within the scope of the above-mentioned embodiment has a lower glass transition temperature (usually between -50°C and -20°C) and better dispersion effect, thus helping to further improve the flexibility and stability of the electrode.
[0046] The hydrogenation degree of the modified nitrile rubber can be achieved by selectively hydrogenating and reducing the double bonds of the diene units to saturated bonds. Therefore, the above hydrogenation degree can also be understood as the proportion of hydrogenated butadiene repeating units in the modified nitrile rubber structure to the total amount of butadiene repeating units.
[0047] The modified nitrile rubber can be prepared by existing processes. In some embodiments, it is prepared by the following method: In a polymerization kettle, butadiene and acrylonitrile monomers are mixed in a certain proportion, and the proportion of acrylonitrile monomer added is controlled to be between 30-40% during the synthesis process, and a free radical polymerization reaction is carried out under the action of an initiator and a catalyst. Specifically, the initiator can be persulfate, potassium persulfate, etc., and the catalyst can be acetic acid ketone, tetrasodium ethylenediaminetetraacetic acid, etc.; the temperature range of the free radical polymerization reaction is between 30°C and 5°C, and the time range is between 2h and 8h. The amount of the initiator added is usually 0.01-2% of the monomer amount; the amount of the catalyst added is usually 5%-10% of the monomer amount.
[0048] In some embodiments, the hydrogenation degree of the modified nitrile rubber can be controlled by adjusting the reaction conditions and the type of catalyst. For example, the modified nitrile rubber (NBR) liquid is added to a stainless steel reactor, the air in the reactor is exhausted, the reactor is heated with stirring to the reaction temperature, a chlorobenzene solution of the catalyst is added, hydrogen is added to a predetermined pressure, the temperature and pressure are maintained constant for different reaction times, and then the pressure is released, the material is cooled and discharged, and condensed with anhydrous ethanol. The material is dried at 60°C to constant weight to obtain modified nitrile rubber (HNBR) with different degrees of hydrogenation. Specifically, the above reaction parameters are listed as follows: the reaction temperature is 80-160°C, hydrogen is added to a hydrogen pressure of 0.05-3Mpa, the reaction time is between 2-10h, and the catalyst can be a homogeneous coordination catalyst of precious metal elements such as palladium, rhodium, and ruthenium and a heterogeneous carrier catalyst, preferably a rhodium-type catalyst.
[0049] In some embodiments, the measurement of the degree of hydrogenation includes the following process: Place the modified nitrile rubber to be measured in a 250 mL iodine flask, add chloroform to dissolve it, then add a quantitative amount of iodine monobromide / carbon tetrachloride solution. After standing for 30 minutes, add potassium iodide solution and distilled water, and titrate with sodium sulfite solution until the solution becomes colorless. Record the volume of sodium sulfite consumed and calculate the degree of hydrogenation.
[0050] In a second aspect, the present invention provides a positive electrode sheet, which includes the binder, positive electrode active material, and conductive agent described in the first aspect.
[0051] Among them, the binder mainly functions to bond the current collector in the positive electrode system. The binder with the polymer material structure of modified nitrile rubber has a certain flexible structure. In a high areal density system, an additional flexible additive is required to play a synergistic effect. Therefore, in order to further increase the areal density of the positive electrode sheet, in an optional embodiment, the polyvinylidene fluoride-based polymer accounts for 3% - 3.5% of the mass of the active material; and / or, the modified nitrile rubber accounts for 0.3% - 0.6% of the mass of the active material.
[0052] Carbon nanotubes can significantly improve the conductivity and mechanical strength of the electrode sheet while maintaining good flexibility. However, the dispersibility of carbon nanotubes is poor and they are prone to agglomeration, which affects the uniformity and flexibility of the electrode sheet. Conductive carbon black not only has good conductivity but also can be evenly distributed in the electrode sheet to form a good conductive network. However, if the addition amount of conductive carbon black is too much, it may cause a decrease in the mechanical strength of the electrode sheet and affect the flexibility. Therefore, in order to ensure that the electrode sheet has both good conductivity and flexibility, in an optional embodiment, the conductive agent includes carbon nanotubes and conductive carbon black; among them, the D50 of the conductive carbon black is 10 nm - 100 nm; the diameter of the carbon nanotubes is 10 nm - 150 nm, and the specific surface area is 10 m 2 / g - 300 m 2 / g.
[0053] Exemplarily, the above-mentioned positive electrode active material is selected from lithium cobaltate (LiCoO2), lithium nickelate (LiNiO2), lithium iron phosphate (LiFePO4), lithium cobalt phosphate (LiCoPO4), lithium manganese phosphate (LiMnPO4), lithium nickel phosphate (LiNiPO4), lithium manganate (LiMnO2), binary material LiNi x A (1-x) O2 (where A is selected from one of Co and Mn, 0 < x < 1), ternary material LiNimBnC (1-m-n)at least one of O2 (wherein B and C are independently selected from at least one of Co, Al, and Mn, and B and C are different, 0 < m < 1, 0 < n < 1); the conductive agent is a material commonly used by those skilled in the art that can enhance electron transport. For example, it can be selected from at least one of natural graphite, artificial graphite, carbon black, acetylene black, Super P, Super S, graphene, carbon fiber, carbon nanotube, and Ketjen black, etc.
[0054] The D50 of the positive electrode active material has a significant impact on the flexibility of the electrode sheet. Small particle size helps to improve the mechanical flexibility and interfacial contact of the electrode sheet, but may increase the processing difficulty and internal resistance; large particle size helps to form a direct conduction path, but may reduce the mechanical flexibility of the electrode sheet. In order to balance the electrochemical performance while improving the flexibility of the electrode sheet, in an optional embodiment, the D50 of the positive electrode active material is 0.30 μm - 0.40 μm.
[0055] In an optional embodiment, the areal density of the positive electrode sheet is 500 g / m 2 -550 g / m 2 ; the tap density is 2.45 - 2.55 g / cm 3 .
[0056] In a specific embodiment, the positive electrode active material is lithium iron phosphate (LFP). When the critical cracking areal density is between 500 - 530 g / m 2 , the addition amount of the polyvinylidene fluoride-based polymer accounts for 3% of the main material, and the conductive agent accounts for about 1.0% of the main material; the addition amount of the modified nitrile rubber accounts for 0.3% - 0.4% of the main material. When the critical cracking areal density is between 530 - 550 g / m 2 , the addition amount of the polyvinylidene fluoride-based polymer accounts for 3.5% of the main material, the addition amount of the conductive agent accounts for about 1.0% of the main material, and the addition amount of the modified nitrile rubber accounts for 0.5% - 0.6% of the main material.
[0057] In a third aspect, the present invention provides a negative electrode sheet, including the binder and the negative electrode active material described in the first aspect.
[0058] Exemplarily, the above negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on at least one surface of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, a conductive agent, and a binder. The negative electrode active material includes one or more of graphite, hard carbon, soft carbon, silicon-based negative electrode, titanium-based material, nitride, stannide, and metallic lithium. The negative electrode current collector can be a conventional negative electrode current collector in the art, such as including copper foil, etc.
[0059] In a fourth aspect, the present invention provides a battery, including the positive electrode sheet described in the second aspect, and / or the negative electrode sheet described in the third aspect.
[0060] The battery of the present invention can be prepared according to conventional methods in the art, such as stacking the positive and negative electrodes and the separator layer together in a certain sequence and rule to form a multi-layer composite film, and then winding it into a cylindrical or square battery cell through a winding process.
[0061] In a specific embodiment, the positive electrode sheet, the separator, and the negative electrode sheet can be stacked in sequence, assembled into a battery cell through a winding process or a stacking process, and then packaged and baked, injected with electrolyte, and then subjected to processes such as hot pressing to obtain a battery.
[0062] The present invention does not specifically limit the above-mentioned separator, and any known porous structure separator with electrochemical stability and chemical stability can be selected, for example, it can be at least one of glass fiber, non-woven fabric, polyethylene, polypropylene or polyvinylidene fluoride. The separator can be single-layer or multi-layer.
[0063] The present invention does not specifically limit the above-mentioned electrolyte, for example, an electrolyte including an organic solvent and an electrolyte salt is selected. Among them, the organic solvent is used as a medium for transmitting ions in the electrochemical reaction, and can be an organic solvent for battery electrolyte known in the art, such as: one or more of fluorinated carbonates, fluorinated carboxylates, non-fluorinated carbonates, fluorinated carbonates, non-fluorinated carboxylates, fluorinated carboxylates, fluorinated carboxylates, fluorinated ethers, non-fluorinated ethers, and tetrahydrofuran; the electrolyte salt is used as a source of ions, and can be an electrolyte salt for battery electrolyte known in the art, such as: one or more of lithium hexafluorophosphate, bistrifluoromethylsulfonyl imide, and bis(fluorosulfonyl)imide lithium.
[0064] It should be noted that the above-mentioned batteries may include but are not limited to single cells, battery modules, battery packs, etc., that is, the actual application form of the battery provided by the present invention can be but is not limited to the listed products, and can also be other application forms. When the battery is a single cell, it includes at least one of a cylindrical battery, a square battery, etc.
[0065] In a fifth aspect, the present invention provides a battery pack comprising the battery described in the fourth aspect.
[0066] In a sixth aspect, the present invention provides an electrical device, comprising the battery described in the fourth aspect or the battery pack described in the fifth aspect.
[0067] It should be noted that the above-mentioned electronic equipment can be any conventional equipment that requires electricity, for example, including but not limited to computers, electric cars, air conditioners, refrigerators, washing machines, microwave ovens, printers, fax machines, etc.
[0068] The present invention is further described below in conjunction with specific embodiments:
[0069] Example 1 This example provides a binder, including a polyvinylidene fluoride-based polymer and a modified nitrile rubber; wherein the modified nitrile rubber has a structure shown in Formula 2, wherein R4 and R6 are C16 linear alkyl chains, and R5 is a C6 linear alkyl chain; The calorific value enthalpy of the polyvinylidene fluoride based polymer is 26 J / g, the polyvinylidene fluoride based polymer is a copolymer of vinylidene fluoride and vinyl carboxylate, and the molecular weight is 800000-2000000 g / mol; the molar content of acrylonitrile in the modified nitrile rubber is 40%; the molecular weight of the modified nitrile rubber is 200000 g / mol-300000 g / mol; and the hydrogenation degree of the modified nitrile rubber is 90%.
[0070] This example also provides a positive electrode sheet, including an aluminum foil with a carbon coating layer (the carbon layer thickness is 1.5µm, the aluminum foil thickness is 14µm) and active material layers on both surfaces of the carbon coating layer, each of the active material layers includes 95 parts of lithium iron phosphate, 1.5 parts of a conductive agent, 3 parts of a polyvinylidene fluoride based polymer and a modified nitrile rubber, the modified nitrile rubber accounts for 0.3wt% of the mass of the lithium iron phosphate, and the conductive agent is carbon nanotubes and carbon black; wherein the D50 particle size of the conductive carbon black is 20nm, the diameter size of the carbon nanotube is 50nm, and the specific surface area is 85m 2 / g, the D50 of lithium iron phosphate is 0.35μm, and the single-sided surface density of the positive electrode is 265g / m 2 , compacted density is 2.45g / cm 3 .
[0071] The preparation process of the positive electrode sheet includes: (1) Add a certain amount of N-methylpyrrolidone (NMP) and add a certain amount of polyvinylidene fluoride polymer powder into the disperser step by step at a speed of 800-1200 rpm. Add while dispersing. Stir for 10-15 minutes at a speed of 800-1200 rpm. Disperse for 30-50 minutes at a speed of 2200-3000 rpm. Pay attention to scraping the edges during the process. Then reduce the dispersion speed to about 1000-1200 rpm. Ensure that there are no bubbles on the surface and no powder flocculation during the dispersion process. The solid content of the system is controlled at 8wt%-10wt%; (2) Add a certain amount of carbon nanotube + carbon black composite conductive slurry to the polyvinylidene fluoride based polymer slurry prepared in step (1), stir at a low speed for 0.5-1.5 hours, adjust the rotation speed during the process, add a certain amount of NMP solvent, and then add different amounts of LFP three times. During the addition process, stir at a low speed for 0.5-1 hour. After the addition is completed, adjust the rotation speed and stir for 1 hour. Then, add modified nitrile rubber under low-speed stirring to obtain a positive electrode slurry.
[0072] (3) The positive electrode slurry is coated on both sides, dried and rolled to obtain the positive electrode sheet.
[0073] Example 2-3 This example provides a binder which differs from Example 1 only in that the calorific value enthalpy of the polyvinylidene fluoride based polymer is changed, as shown in Table 1; This example also provides a positive electrode sheet, which is different from Example 1 only in that the binder is replaced with the above-mentioned binder.
[0074] Embodiment 4-6 A binder and a positive electrode sheet are provided respectively, which are different from Example 1 only in that: the modified nitrile rubber has a structure shown in Formula 1, wherein R1 and R3 are straight-chain alkyl chains of C12, and R3 is a straight-chain alkyl chain of C6; and the calorific value enthalpy of the polyvinylidene fluoride based polymer is changed, as shown in Table 1.
[0075] Example 7 The binder and positive electrode provided in this example are different from those in Example 1 only in that modified nitrile rubber is not included.
[0076] The preparation of the positive electrode sheet comprises the following steps: The invention comprises an aluminum foil containing a carbon coating layer (the thickness of the carbon layer is 1.5 µm, and the thickness of the aluminum foil is 14 µm) and active material layers on both surfaces of the carbon coating layer, wherein the active material layer comprises 95 parts of lithium iron phosphate, 1.5 parts of a conductive agent, and 3.2 parts of a polyvinylidene fluoride based polymer, and the conductive agent is a carbon nanotube and carbon black; wherein the D50 particle size of the conductive carbon black is 20 nm, the diameter size of the carbon nanotube is 50 nm, and the specific surface area is 85 m 2 / g, the D50 of lithium iron phosphate is 0.35μm, and the single-sided surface density of the positive electrode is 265g / m 2 , compacted density is 2.45g / cm 3 .
[0077] The preparation process of the above-mentioned positive electrode sheet includes: (1) Add a certain amount of N-methylpyrrolidone (NMP) and add a certain amount of polyvinylidene fluoride polymer powder into the disperser step by step at a speed of 800-1200 rpm. Add while dispersing. Stir for 10-15 minutes at a speed of 800-1200 rpm. Disperse for 30-50 minutes at a speed of 2200-3000 rpm. Pay attention to scraping the edges during the process. Then reduce the dispersion speed to about 1000-1200 rpm. Ensure that there are no bubbles on the surface and no powder flocculation during the dispersion process. The solid content of the system is controlled at 8wt%-10wt%; (2) Add a certain amount of carbon nanotube + carbon black composite conductive slurry to the polyvinylidene fluoride based polymer slurry prepared in step (1), stir at a low speed for 0.5-1.5 hours, adjust the rotation speed during the process, add a certain amount of NMP solvent, and then add different amounts of LFP three times. During the addition process, stir at a low speed for 0.5-1 hour. After the addition is completed, adjust the rotation speed, stir for 1 hour, and then stir at a low speed to obtain the positive electrode slurry after caching.
[0078] (3) The positive electrode slurry is coated on both sides, dried and rolled to obtain the positive electrode sheet.
[0079] Example 8 The binder and positive electrode provided in this example are different from those in Example 1 only in that the binder is composed of modified nitrile rubber consistent with that in Example 1 and polyvinylidene fluoride having a calorific value enthalpy of 42 J / g.
[0080] The preparation of the positive electrode sheet comprises the following steps: The invention comprises an aluminum foil containing a carbon coating layer (the thickness of the carbon layer is 1.5µm, and the thickness of the aluminum foil is 14µm) and active material layers on both surfaces of the carbon coating layer, wherein the active material layer comprises 95 parts of lithium iron phosphate, 1.5 parts of a conductive agent, 3.2 parts of a polyvinylidene fluoride polymer and a modified nitrile rubber, wherein the modified nitrile rubber accounts for 0.5wt% of the mass of the lithium iron phosphate, and the conductive agent is carbon nanotubes and carbon black; wherein the D50 particle size of the conductive carbon black is 20nm, the diameter size of the carbon nanotubes is 50nm, and the specific surface area is 85m 2 / g, the D50 of lithium iron phosphate is 0.35μm, and the single-sided surface density of the positive electrode is 265g / m 2 , compacted density is 2.45g / cm 3 .
[0081] The preparation process of the above-mentioned positive electrode sheet includes: (1) Add a certain amount of N-methylpyrrolidone (NMP) and add a certain amount of polyvinylidene fluoride polymer powder into the disperser step by step at a speed of 800-1200rpm. Add while dispersing. Stir for 10-15min at a speed of 800-1200rpm. Disperse for 30-50min at a speed of 2200-3000rpm. Pay attention to scraping the edges during the process. Then reduce the dispersion speed to about 1000-1200rpm. Ensure that there are no bubbles on the surface and no powder flocculation during the dispersion process. The solid content of the system is controlled at 8wt%-10wt%; (2) Add a certain amount of carbon nanotube + carbon black composite conductive slurry to the polyvinylidene fluoride polymer slurry prepared in step (1), stir at a low speed for 0.5-1.5 hours, adjust the speed during the process, add a certain amount of NMP solvent, and then add different amounts of LFP three times. During the addition process, stir at a low speed for 0.5-1 hour. After the addition is completed, adjust the speed and stir for 1 hour. Then, add modified nitrile rubber under low-speed stirring to obtain a positive electrode slurry.
[0082] (3) The positive electrode slurry is coated on both sides, dried and rolled to obtain the positive electrode sheet.
[0083] Comparative Examples 1-3 The provided binder and positive electrode sheet differ from those in Example 1 only in that the binder is polyvinylidene fluoride, and its calorific value enthalpy is shown in Table 1.
[0084] Test Case The flexibility test of the pole pieces of the embodiment and the comparative example is as follows: 1) Use the bending machine equipment, set the parameters: left-hand angle 90 degrees, right-hand angle 90 degrees, the running speed is maintained at 50 times / min, and the number of times is set to the dynamic range; 2) Place the electrode to be tested on the fixture and keep it in a vertical position; 3) Press the start button to record the number of bending times of the critical fracture of the pole piece; 4) The final bending times data is used to judge the performance of flexibility. The more times, the better the fatigue resistance of the pole piece. If the pole piece does not break during the bending process for more than 200 times, it can be considered that the flexibility of the pole piece has reached the best level. 100-200 times, the flexibility level is medium, and less than 100 times, the flexibility level is poor.
[0085] The results of the flexibility of the pole pieces of the embodiments and comparative examples are shown in Table 1, where: Figure 1 In the comparative example 1, the pole piece without the addition of the flexibilizer material was broken after about 10-15 times of the bending resistance test. Figure 2 The pole piece in Example 1 with flexible material added did not break after more than 100 times.
[0086] The calorific value enthalpy of the polyvinylidene fluoride based polymer of Example 1 and Comparative Example 1 was tested by differential scanning calorimetry. The testing process included: a first stage temperature scanning range, 10.0°C / min to 200.0°C; a second stage, a heat preservation time of -30.0°C; a third stage temperature scanning range, 10.0°C / min to 200.0°C. The test results are shown in FIG. Figure 3 .
[0087] Table 1:
[0088] It can be seen from Table 1 that, compared with the comparative example, the pole piece of the embodiment can significantly improve its flexibility without reducing the pole piece surface density and compaction.
[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A binder, characterized in that: It includes modified nitrile rubber and / or polyvinylidene fluoride based polymer; the modified nitrile rubber includes the structure shown in Formula 1 and / or Formula 2: Formula 1, Formula 2, In Formula 1, R1 and R3 are each independently an alkyl chain greater than or equal to C8, R2 is an alkyl chain greater than or equal to C6, and x is greater than or equal to 1; In Formula 2, R4 and R6 are each independently an alkyl chain of C8 or greater, R5 is an alkyl chain of C6 or greater, and x is greater than or equal to 1; The calorific value enthalpy of the polyvinylidene fluoride-based polymer is less than or equal to 30 J / g.
2. The adhesive according to claim 1, characterized in that In formula 1, R1 and R3 are each independently a branched alkyl chain of C8-C60 or a branched alkyl chain, and R2 is a branched alkyl chain of C6-C30 or a branched alkyl chain; in formula 2, R4 and R6 are each independently a branched alkyl chain of C8-C60 or a branched alkyl chain, and R5 is a branched alkyl chain of C6-C30 or a branched alkyl chain.
3. The adhesive according to claim 1, characterized in that The calorific value enthalpy of the polyvinylidene fluoride-based polymer is greater than or equal to 15 J / g.
4. The adhesive according to claim 1, characterized in that The polyvinylidene fluoride based polymer is selected from a mixture of polyvinylidene fluoride and a second polymer, wherein the second polymer is at least one of polyethylene glycol, polymethyl methacrylate, and polyvinyl acetate; And / or, the polyvinylidene fluoride-based polymer is selected from a copolymer of vinylidene fluoride and a second monomer, and the second monomer is vinyl carboxylate, ethylene glycol oxalate or ethylene glycol succinate.
5. The adhesive according to any one of claims 1 to 4, characterized in that: The molar content of acrylonitrile in the modified nitrile rubber is 30%-40%; And / or, the molecular weight of the modified nitrile rubber is 200000 g / mol-300000 g / mol; And / or, the degree of hydrogenation of the modified nitrile rubber is 90%-99%.
6. A positive electrode sheet, characterized in that: The invention comprises the binder according to any one of claims 1 to 5, a positive electrode active material and a conductive agent.
7. The positive electrode sheet according to claim 6, characterized in that: The polyvinylidene fluoride based polymer accounts for 3% to 3.5% of the mass of the positive electrode active material; And / or, the modified nitrile rubber accounts for 0.3%-0.6% of the mass of the positive electrode active material.
8. The positive electrode sheet according to claim 6, characterized in that: The conductive agent includes carbon nanotubes and conductive carbon black; wherein the D 50 The carbon nanotube has a diameter of 10 nm to 150 nm and a specific surface area of 10 m 2 / g-300m 2 / g.
9. The positive electrode sheet according to claim 7, characterized in that: The D50 of the positive electrode active material is 0.30 μm-0.40 μm.
10. The positive electrode sheet according to any one of claims 6 to 9, characterized in that: The surface density of the positive electrode sheet is 500g / m 2 -550g / m 2 ; compacted density is 2.45g / cm 3 -2.55g / cm 3 .
11. A negative electrode sheet, characterized in that: The invention comprises the binder and the negative electrode active material as described in any one of claims 1 to 5.
12. A battery, characterized in that: It comprises the positive electrode sheet as described in any one of claims 6 to 10, and / or the negative electrode sheet as described in claim 11.
13. A battery pack, characterized in that: Comprising the battery as claimed in claim 12.
14. An electrical device, characterized in that: Includes the battery according to claim 12 or the battery pack according to claim 13.
Citation Information
Patent Citations
Fluorine-containing polymer, preparation method and application thereof, binder composition, secondary battery, battery module, battery pack and electric device
CN115124638A
Fluorine-containing polymer, preparation method, positive pole piece, secondary battery and electric device
CN116715798A
Modified binder, positive electrode slurry, positive plate and lithium ion battery
CN117363264A
Negative electrode slurry and preparation method thereof, negative electrode plate and lithium titanate battery
CN118156462A
Lithium ion battery, preparation method thereof, positive pole piece and power utilization device
CN118712459A