Long-open water-based adhesive and application thereof

By adding vinyl aqueous emulsion polymer, fast conjunctiva sealing additive and infrared light heat quickly absorbing and heating materials to the adhesive, using infrared light heating technology, the problems of slow curing speed of the adhesive and insufficient opening time of the aqueous adhesive are solved, and rapid Curing and efficient production improve product quality and production efficiency.

CN119019957APending Publication Date: 2024-11-26DINGLI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411272468.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing adhesives have low absorption efficiency of infrared light, resulting in slow curing and heating up speed. The water-based adhesives are insufficient to open during the heating process, resulting in false stickiness and cracking of the product, and long pressurization and health preservation time in winter, affecting production efficiency.

Method used

Long open water-based adhesives are used, including vinyl aqueous emulsion polymers, rapid conjunctiva sealing additives and infrared light heat-absorbing and heating materials, and rapid curing is achieved through infrared light heating, and infrared heat-cured composite panels are formed in combination with cold pressing.

Benefits of technology

It significantly improves the curing speed of the adhesive, improves product performance, shortens drying time, improves production efficiency, avoids false sticking and cracking, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a long-open water-based adhesive and application thereof. The long-open water-based adhesive comprises a vinyl water-based emulsion polymer, a rapid conjunctival sealing aid and an infrared light heat rapid absorption heating material. A wooden board A and a wooden board B which are to be bonded are cleaned and then dried, the A is coated with an adhesive, then the A is placed under an infrared light heating device to be heated, after the A is heated to the target range temperature, the wooden board A is taken out, the wooden board A and the wooden board B are closed and wait, and a composite board intermediate A is formed; and placing the wood composite board intermediate A under a flat plate cold press, and carrying out cold pressing for several minutes to obtain the infrared thermocuring composite board. The long-open water-based adhesive provided by the invention has no adverse effect on human health and environment, has excellent infrared radiation absorption performance and can rapidly seal adhesive film moisture, so that the emulsion adhesive is rapidly heated before emulsion particles form a film; the temperature of the wooden board and the adhesive layer can be quickly and uniformly increased, the energy consumption is reduced, the cold pressing time is greatly shortened, the curing efficiency is improved, and the technical problems of false adhesion and cracking of the wooden composite board caused by quick moisture evaporation of the adhesive can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an adhesive preparation technology, in particular to a long-release water-based adhesive and application thereof. Background Art

[0002] In the field of wood processing technology, adhesive is an important auxiliary material that can make the connection between woods tighter and improve the stability and durability of the product. However, traditional adhesives usually need to be cured by heating, which is not only time-consuming but also consumes a lot of energy. In order to solve this problem, infrared light curing technology came into being. It can cure adhesives quickly in a short time through infrared irradiation, greatly improving production efficiency.

[0003] Solutions of existing technologies: Existing solutions are mainly to change the formula of adhesives or adjust the curing conditions, such as increasing the curing agent content in the adhesive, or increasing the curing temperature and time. In addition, there are some methods to change the form of adhesives, such as using hot melt adhesives or UV adhesives, which can be quickly cured at room temperature, thereby improving production efficiency.

[0004] Problems with existing technologies: Although existing technologies have solved the problem of slow curing of adhesives to a certain extent, they also have some problems and shortcomings. First, the existing adhesives have low absorption efficiency of infrared light, resulting in a relatively slow curing temperature rise rate. Second, the open time of water-based adhesives during the heating process needs to be improved, which will cause false adhesion and cracking of the product. Finally, because the water-based adhesive evaporates slowly, the pressurization time and curing time in winter are long, which greatly limits the production efficiency of the factory.

[0005] Compared with the prior art, the present invention solves the following problems: 1) The absorption efficiency of infrared light by adhesive is not high, resulting in a slow curing temperature rise rate; 2) The open time of water-based adhesive during heating needs to be improved, which will cause false adhesion and cracking of the product; 3) Overcoming the technical problem that water-based adhesive has slow evaporation of water and long pressurization and curing time in winter. Summary of the invention

[0006] The purpose of the present invention is to provide a long-open water-based adhesive and application thereof in view of the deficiencies in the prior art.

[0007] The objective of the present invention is achieved through the following technical solutions:

[0008] In a first aspect, the present invention provides a long-open water-based adhesive comprising the following components:

[0009] 60-90 parts by weight of vinyl aqueous emulsion polymer

[0010] 1-10 parts by weight of rapid conjunctival sealing aid

[0011] The infrared light heat fast absorbing and heating material comprises 5 to 30 parts by weight.

[0012] Furthermore, the vinyl water-based emulsion polymer is a mixture of two or more of polyvinyl alcohol solution, polyvinyl acetate emulsion, vinyl acetate-ethylene copolymer emulsion, vinyl acetate-acrylate copolymer emulsion, and vinyl acetate-versatate copolymer emulsion in any proportion.

[0013] Furthermore, the rapid conjunctival sealing aid is composed of two or more of acrylamide-acrylate polymer, plasticizer, film-forming aid, hydroxyethyl urea, vaseline, semi-refined paraffin, and glycerin mixed in any proportion.

[0014] Furthermore, the infrared light heat rapid absorption and temperature rise material is composed of two or more of carbon nanotube material, carbon black, carboxylated graphene oxide surface grafted polylactic acid composite, titanium dioxide, four-arm star-shaped polyethylene glycol modified graphene oxide, zinc oxide, antimony tin oxide, artificial corundum, and silicon carbide mixed in any proportion.

[0015] In a second aspect, the present invention provides an application of a long-open water-based adhesive, wherein the long-open water-based adhesive can be used to prepare an infrared heat-cured composite board.

[0016] Furthermore, the application includes the following specific steps:

[0017] (1) wooden board A and wooden board B are cleaned and dried respectively; a long-open water-based adhesive is coated on the dried wooden board A, and then heated under an infrared heating device;

[0018] (2) After the wooden board A is heated to 35-65° C., the wooden board A and the wooden board B are closed, and after waiting for 1-5 minutes, a composite board intermediate C is obtained;

[0019] (3) The composite board intermediate C is placed under a flat cold press and cold pressed for 1 to 2 minutes to obtain an infrared heat-cured composite board.

[0020] Furthermore, the infrared light heating device is an infrared lamp with a power of 1000W and a wavelength range of 700-1500nm.

[0021] Furthermore, in step (3), the pressure to be applied in the cold pressing is 80 psi to 500 psi.

[0022] Furthermore, the wooden board A and wooden board B are hardwood plywood, softwood plywood, particle board, medium density fiberboard, oriented strand board, waffle board, fiberboard, parallel plywood, shavings laminated timber or hardwood veneer products respectively.

[0023] The beneficial effects of the present invention are:

[0024] 1) Improve the curing speed: By optimizing the adhesive formula and introducing infrared light curing equipment, we can significantly increase the curing speed of water-based wood adhesives, allowing the latex adhesive to heat up quickly before the latex particles aggregate into a film, thereby improving the factory's production efficiency; this is something that existing technologies cannot do;

[0025] 2) Improve product performance: By adopting the form of double-sided thickening of single-board glue coating, we can avoid false adhesion and cracking of products, and improve the quality and stability of products; this is impossible to achieve by changing the form of adhesive in the prior art;

[0026] 3) Shorten the drying time: During the drying process, we can raise the temperature of the water-based adhesive to above 50°C in a short time through infrared light irradiation, reduce the cold pressing time to less than 2 minutes, greatly shorten the pressing time and curing time in winter, and further improve production efficiency; this is something that cannot be achieved by changing the curing conditions in the prior art;

[0027] 4) In general, compared with the prior art, the present invention not only improves the curing speed of the adhesive and improves the performance of the product, but also shortens the drying time, and has obvious advantages. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in combination with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In order to overcome the deficiencies of the above-mentioned prior art, the present invention proposes a method for infrared light thermal curing of wood product adhesives, which mainly solves the technical problem that the adhesive has low absorption efficiency of infrared light, resulting in a relatively slow curing temperature rise rate; solves the technical problem that the water-based adhesive has a short open time during the heating process and is prone to film formation and surface drying, which will cause false adhesion and cracking of the product; overcomes the technical problem that the water-based adhesive has slow evaporation of water and long pressurization time and curing time in winter, and can quickly and evenly increase the temperature of the wooden board and the glue layer, shorten the preparation time, reduce energy consumption, and thereby improve the bonding strength of the wooden board.

[0030] The present invention provides a long-open water-based adhesive, comprising the following components:

[0031] 60-90 parts by weight of vinyl aqueous emulsion polymer

[0032] 1-10 parts by weight of rapid conjunctival sealing aid

[0033] The infrared light heat fast absorbing and heating material comprises 5 to 30 parts by weight.

[0034] The vinyl water-based emulsion polymer is a mixture of two or more of polyvinyl alcohol solution, polyvinyl acetate emulsion, vinyl acetate-ethylene copolymer emulsion, vinyl acetate-acrylate copolymer emulsion, and vinyl acetate-versatate copolymer emulsion in any proportion.

[0035] The rapid conjunctival sealing aid is composed of two or more of acrylamide-acrylate polymer, plasticizer, film-forming aid, hydroxyethyl urea, vaseline, semi-refined paraffin and glycerol mixed in any proportion.

[0036] The infrared light heat rapid absorption and temperature-raising material is composed of two or more of carbon nanotube material, carbon black, carboxylated graphene oxide surface grafted polylactic acid composite (GO-COOH-PLLA-PEG-PLLA), titanium dioxide, four-arm star-shaped polyethylene glycol modified graphene oxide (GO-TDI-sPEG), zinc oxide, antimony tin oxide, artificial corundum, and silicon carbide mixed in any proportion.

[0037] The invention also provides the use of the long-open water-based adhesive in preparing infrared heat-curing composite panels.

[0038] The application includes the following specific steps:

[0039] (1) wooden board A and wooden board B are cleaned and dried respectively; a long-open water-based adhesive is coated on the dried wooden board A, and then heated under an infrared heating device;

[0040] (2) After the wooden board A is heated to 35-65° C., the wooden board A and the wooden board B are closed, and after waiting for 1-5 minutes, a composite board intermediate C is obtained;

[0041] (3) The composite board intermediate C is placed under a flat cold press and cold pressed for 1 to 2 minutes to obtain an infrared heat-cured composite board.

[0042] The infrared light heating device is an infrared lamp with a power of 1000W and a wavelength range of 700-1500nm.

[0043] In step (3), the pressure to be applied in the cold pressing is 80 psi to 500 psi.

[0044] The wooden board A and wooden board B are hardwood plywood, softwood plywood, particle board, medium density fiberboard, oriented strand board, waffle board, fiberboard, parallel plywood, shavings laminated timber or hardwood veneer products respectively.

[0045] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0046] Example 1

[0047] Preparation of a long-open water-based adhesive:

[0048] A vinyl water-based emulsion polymer composed of a polyvinyl acetate emulsion and a polyvinyl alcohol solution in a mass ratio of 5:1, a rapid conjunctival sealing aid composed of a semi-refined paraffin, a plasticizer and hydroxyethyl urea in a mass ratio of 1:1:1, and an infrared light heat rapid absorption and heating material composed of carbon black, a carboxylated graphene oxide surface grafted polylactic acid composite and artificial corundum in a mass ratio of 10:1:10 were selected, and then the vinyl water-based emulsion polymer, the rapid conjunctival sealing aid and the infrared light heat rapid absorption and heating material were mixed in a mass ratio of 80:5:15. A high-speed stirrer was used for mixing, the speed was set to 1000 rpm, and the stirring time was 30 minutes to ensure sufficient mixing of the three materials and to ensure that the glue had no obvious particles, so as to obtain a long-open water-based adhesive.

[0049] Preparation of infrared heat-cured composite panels:

[0050] (1) The cork plywood and the medium density fiberboard are cleaned and dried respectively; a long-open water-based adhesive is coated on the dried cork plywood, and then heated under an infrared heating device.

[0051] In this embodiment, an infrared light heating device is introduced: a 1000W infrared lamp is used, the wavelength range is 700-1500nm, and the irradiation time is 80 seconds. During the curing process, the ambient temperature is 15°C and the humidity is 60% to ensure the best curing effect.

[0052] (2) After the wooden board A is heated to 65° C., the cork plywood is taken out, and the heated cork plywood and the medium-density fiberboard are closed, and a composite board intermediate C is obtained after waiting for 1 minute.

[0053] (3) The composite board intermediate C is placed under a flat cold press, a pressure of 300 Psi is applied, and cold pressing is performed for 1 min to obtain an infrared heat-cured composite board.

[0054] Testing of infrared heat-cured composite panels:

[0055] With reference to "Surface bonding strength determination - Method 1" in GB / T17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels", a tensile testing machine was used to fix both sides of the infrared heat-cured composite panel prepared in Example 1, and a tensile test was performed on the infrared heat-cured composite panel using a tensile testing machine. The test results showed that the bonding strength was 2.2 MPa.

[0056] Example 2

[0057] Preparation of a long-open water-based adhesive:

[0058] A vinyl water-based emulsion polymer composed of a polyvinyl acetate emulsion and a vinyl acetate-acrylate copolymer emulsion in a mass ratio of 6:1, a rapid conjunctival sealing adjuvant composed of a semi-refined paraffin wax, a plasticizer and glycerol in a mass ratio of 1:2:1, and an infrared light heat rapid absorption and heating material composed of a carboxylated graphene oxide surface grafted polylactic acid composite, a four-arm star-shaped polyethylene glycol-modified graphene oxide and silicon carbide in a mass ratio of 20:1:1 were selected, and then the vinyl water-based emulsion polymer, the rapid conjunctival sealing adjuvant and the infrared light heat rapid absorption and heating material were mixed in a mass ratio of 90:3:7. A high-speed stirrer was used for mixing, the speed was set to 1000 rpm, and the stirring time was 30 minutes to ensure that the three materials were fully mixed and that the glue had no obvious particles, so as to obtain a long-open water-based adhesive.

[0059] Preparation of infrared heat-cured composite panels:

[0060] (1) The shavings and medium density fiberboard are cleaned and dried respectively; a long-open water-based adhesive is coated on the dried shavings and then heated under an infrared heating device.

[0061] In this embodiment, an infrared light heating device is introduced: a 1000W infrared lamp is used, the wavelength range is 700-1500nm, and the irradiation time is 60 seconds. During the curing process, the ambient temperature is 20°C and the humidity is 80% to ensure the best curing effect.

[0062] (2) After the wooden board A is heated to 55° C., the shavings laminated material is taken out, and the heated shavings laminated material is closed with the medium-density fiberboard, and a composite board intermediate C is obtained after waiting for 3 minutes.

[0063] (3) The composite board intermediate C is placed under a flat cold press, a pressure of 400 Psi is applied, and cold pressing is performed for 2 minutes to obtain an infrared heat-cured composite board.

[0064] Testing of infrared heat-cured composite panels:

[0065] With reference to "Surface bonding strength determination - Method 1" in GB / T17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels", a tensile testing machine was used to fix both sides of the infrared heat-cured composite panel prepared in Example 2, and a tensile test was performed on the infrared heat-cured composite panel using a tensile testing machine. The test results showed that the bonding strength was 1.8 MPa.

[0066] Example 3

[0067] Preparation of a long-open water-based adhesive:

[0068] A vinyl water-based emulsion polymer composed of a polyvinyl alcohol solution and a vinyl acetate-ethylene copolymer emulsion in a mass ratio of 3:2, a rapid conjunctival sealing aid composed of vaseline, a plasticizer and glycerin in a mass ratio of 1:3:2, and an infrared light heat rapid absorption and heating material composed of a carboxylated graphene oxide surface grafted polylactic acid composite, a four-arm star-shaped polyethylene glycol modified graphene oxide and silicon carbide in a mass ratio of 1:1:18 were selected, and then the vinyl water-based emulsion polymer, the rapid conjunctival sealing aid and the infrared light heat rapid absorption and heating material were mixed in a mass ratio of 65:10:25. A high-speed stirrer was used for mixing, the speed was set to 1000 rpm, and the stirring time was 30 minutes to ensure that the three materials were fully mixed and that the glue had no obvious particles, so as to obtain a long-open water-based adhesive.

[0069] Preparation of infrared heat-cured composite panels:

[0070] (1) The shavings and medium density fiberboard are cleaned and dried respectively; a long-open water-based adhesive is coated on the dried shavings and then heated under an infrared heating device.

[0071] In this embodiment, an infrared light heating device is introduced: a 1000W infrared lamp is used, the wavelength range is 700-1500nm, and the irradiation time is 120 seconds. During the curing process, the ambient temperature is -5°C and the humidity is 20% to ensure the best curing effect.

[0072] (2) After the wooden board A is heated to 65° C., the shavings laminated material is taken out, and the heated shavings laminated material is closed with the medium-density fiberboard. After waiting for 1 minute, a composite board intermediate C is obtained.

[0073] (3) The composite board intermediate C is placed under a flat cold press, a pressure of 100 Psi is applied, and cold pressing is performed for 1 minute to obtain an infrared heat-cured composite board.

[0074] Testing of infrared heat-cured composite panels:

[0075] With reference to "Surface bonding strength determination - Method 1" in GB / T17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels", a tensile testing machine was used to fix both sides of the infrared heat-cured composite panel prepared in Example 3, and a tensile test was performed on the infrared heat-cured composite panel using a tensile testing machine. The test results showed that the bonding strength was 1.63 MPa.

[0076] Example 4

[0077] Preparation of a long-open water-based adhesive:

[0078] A vinyl water-based emulsion polymer composed of a polyvinyl alcohol solution and a vinyl acetate-versatate copolymer emulsion in a mass ratio of 1:2, a rapid conjunctival sealing aid composed of semi-refined paraffin, a plasticizer and glycerin in a mass ratio of 1:3:2, and an infrared light heat rapid absorption and heating material composed of an artificial corundum and a carboxylated graphene oxide surface grafted polylactic acid composite in a mass ratio of 1:2 were selected, and then the vinyl water-based emulsion polymer, the rapid conjunctival sealing aid and the infrared light heat rapid absorption and heating material were mixed in a mass ratio of 85:5:10. A high-speed stirrer was used for mixing, the speed was set to 1000 rpm, and the stirring time was 30 minutes to ensure sufficient mixing of the three materials and to ensure that the glue had no obvious particles, so as to obtain a long-open water-based adhesive.

[0079] Preparation of infrared heat-cured composite panels:

[0080] (1) The medium density fiberboard and the medium density fiberboard are cleaned and dried respectively; a long-open water-based adhesive is coated on the dried medium density fiberboard, and then heated under an infrared light heating device.

[0081] In this embodiment, an infrared light heating device is introduced: a 1000W infrared lamp is used, the wavelength range is 700-1500nm, and the irradiation time is 30 seconds. During the curing process, the ambient temperature is 10°C and the humidity is 80% to ensure the best curing effect.

[0082] (2) After the wooden board A is heated to 45° C., the medium density fiberboard is taken out, and the heated medium density fiberboard and the medium density fiberboard are closed together, and a composite board intermediate C is obtained after waiting for 5 minutes.

[0083] (3) The composite board intermediate C is placed under a flat cold press, a pressure of 500 Psi is applied, and cold pressing is performed for 1 min to obtain an infrared heat-cured composite board.

[0084] Testing of infrared heat-cured composite panels:

[0085] With reference to "Surface bonding strength determination - Method 1" in GB / T17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels", a tensile testing machine was used to fix both sides of the infrared heat-cured composite panel prepared in Example 4, and a tensile test was performed on the infrared heat-cured composite panel using a tensile testing machine. The test results showed that the bonding strength was 1.87 MPa.

[0086] Comparative Example 1

[0087] Preparation of a long-open water-based adhesive:

[0088] A vinyl water-based emulsion polymer composed of a polyvinyl alcohol solution and a polyvinyl acetate emulsion in a mass ratio of 1:3, a rapid conjunctival sealing adjuvant composed of a plasticizer and glycerin in a mass ratio of 1:1, and an infrared light heat rapid absorption and heating material composed of zinc oxide and antimony tin oxide in a mass ratio of 1:1 were selected, and then the vinyl water-based emulsion polymer, the rapid conjunctival sealing adjuvant and the infrared light heat rapid absorption and heating material were mixed in a mass ratio of 97:2:1. A high-speed stirrer was used for mixing, the speed was set to 1000 rpm, and the stirring time was 30 minutes to ensure sufficient mixing of the three materials and to ensure that the glue had no obvious particles, so as to obtain a long-open water-based adhesive.

[0089] Preparation of infrared heat-cured composite panels:

[0090] (1) The medium density fiberboard and the medium density fiberboard are cleaned and dried respectively; a long-open water-based adhesive is coated on the dried medium density fiberboard, and then heated under an infrared light heating device.

[0091] In this embodiment, an infrared light heating device is introduced: a 1000W infrared lamp is used, the wavelength range is 700-1500nm, and the irradiation time is 60 seconds. During the curing process, the ambient temperature is 10°C and the humidity is 80% to ensure the best curing effect.

[0092] (2) After the wooden board A is heated to 45° C., the medium density fiberboard is taken out, and the heated medium density fiberboard and the medium density fiberboard are closed together, and a composite board intermediate C is obtained after waiting for 5 minutes.

[0093] (3) The composite board intermediate C is placed under a flat cold press, a pressure of 500 Psi is applied, and cold pressing is performed for 2 minutes to obtain an infrared heat-cured composite board.

[0094] Testing of infrared heat-cured composite panels:

[0095] With reference to "Surface Bonding Strength Determination - Method 1" in GB / T17657-2013 "Test Methods for Physical and Chemical Properties of Artificial Boards and Faced Artificial Boards", a tensile testing machine was used to fix both sides of the infrared heat-cured composite board prepared in Comparative Example 1, and a tensile test was performed on the infrared heat-cured composite board using a tensile testing machine. The test results showed that the bonding strength was 0.87 MPa.

[0096] Comparative Example 2

[0097] Take a conventional PVAc emulsion water-based adhesive on the market with a solid content of 50% as an adhesive for later use.

[0098] Preparation of infrared heat-cured composite panels:

[0099] (1) The medium density fiberboard and the medium density fiberboard are cleaned and dried respectively; the dried medium density fiberboard is coated with adhesive and then heated under an infrared light heating device.

[0100] In this embodiment, an infrared light heating device is introduced: a 1000W infrared lamp is used, the wavelength range is 700-1500nm, and the irradiation time is 80 seconds. During the curing process, the ambient temperature is 10°C and the humidity is 60% to ensure the best curing effect.

[0101] (2) After the wooden board A is heated to 40° C., the medium density fiberboard is taken out, and the heated medium density fiberboard and the medium density fiberboard are closed, and after waiting for 2 minutes, a composite board intermediate C is obtained;

[0102] (3) The composite board intermediate C is placed under a flat cold press, a pressure of 500 Psi is applied, and cold pressing is performed for 2 minutes to obtain an infrared heat-cured composite board.

[0103] Testing of infrared heat-cured composite panels:

[0104] With reference to "Surface Bonding Strength Determination - Method 1" in GB / T17657-2013 "Test Methods for Physical and Chemical Properties of Artificial Boards and Faced Artificial Boards", a tensile testing machine was used to fix both sides of the infrared heat-cured composite board prepared in Comparative Example 2, and a tensile test was performed on the infrared heat-cured composite board using a tensile testing machine. The test results showed that the bonding strength was 0.58 MPa.

[0105] The infrared heat-curing composite panels prepared in Examples 1 to 4 and the infrared heat-curing composite panels prepared in Comparative Examples 1 and 2 were tested for performance indicators. The test results are shown in Table 1.

[0106] Table 1: Performance index test results

[0107] Test items Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Appearance grey grey grey grey milky milky Solid content by mass (%) 45% 35% 50% 40% 50% 50% Viscosity(mpa.s) 23500 25000 25500 26000 25000 25000 Light exposure time (seconds) 80 60 120 30 60 80 Ambient temperature 15 20 -5 10 10 10 Heating plate A temperature 65 55 75 45 45 40 Closing waiting time 1 3 1 5 2 2 Applied pressure (psi) 100 300 500 200 200 200 Bonding strength(Mpa) 2.2 1.8 1.63 1.87 0.87 0.58

[0108] In summary, the method of using the infrared curing wood product adhesive of the present invention can quickly and evenly increase the temperature of the wooden board and each adhesive layer, shorten the preparation time, reduce energy consumption, and improve the curing efficiency; the infrared light heat is used to quickly absorb the heating material, and the rapid sealing film moisture additive is introduced, so that the wooden board is coated with the adhesive to the maximum extent, and the latex adhesive is quickly heated before the latex particles form a film, so as to achieve the effect of rapid hot pressing. However, the glue without the introduction of the rapid film-binding sealing additive will continue to evaporate the water after the wooden board is coated with the adhesive and heated, resulting in false stickiness of the product; the purchased water-based adhesive also has a slow heating speed and poor initial viscosity because it does not introduce the infrared light heat to quickly absorb the heating material and the rapid film-binding sealing additive, and cannot reach the ideal rapid pressure relief strength.

[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A long-release water-based adhesive, characterized in that: The components include: 60-90 parts by weight of vinyl aqueous emulsion polymer 1-10 parts by weight of rapid conjunctival sealing aid The infrared light heat fast absorbing heating material comprises 5 to 30 parts by weight.

2. A long-release water-based adhesive according to claim 1, characterized in that: The vinyl water-based emulsion polymer is a mixture of two or more of polyvinyl alcohol solution, polyvinyl acetate emulsion, vinyl acetate-ethylene copolymer emulsion, vinyl acetate-acrylate copolymer emulsion, and vinyl acetate-versatate copolymer emulsion in any proportion.

3. A long-open water-based adhesive according to claim 1, characterized in that: The rapid conjunctival sealing aid is composed of two or more of acrylamide-acrylate polymer, plasticizer, film-forming aid, hydroxyethyl urea, vaseline, semi-refined paraffin and glycerol mixed in any proportion.

4. The long-release water-based adhesive according to claim 1, characterized in that: The infrared light heat rapid absorption and temperature-raising material is composed of two or more of carbon nanotube material, carbon black, carboxylated graphene oxide surface grafted polylactic acid composite, titanium dioxide, four-arm star-shaped polyethylene glycol modified graphene oxide, zinc oxide, antimony tin oxide, artificial corundum, and silicon carbide mixed in any proportion.

5. An application of the long-open water-based adhesive according to claim 1, characterized in that: The long-open water-based adhesive can be used to prepare infrared heat-cured composite panels.

6. The use according to claim 5, characterized in that: The application includes the following specific steps: (1) wooden board A and wooden board B are cleaned and dried respectively; a long-open water-based adhesive is coated on the dried wooden board A, and then heated under an infrared heating device; (2) After the wooden board A is heated to 35-65° C., the wooden board A and the wooden board B are closed, and after waiting for 1-5 minutes, a composite board intermediate C is obtained; (3) The composite board intermediate C is placed under a flat cold press and cold pressed for 1 to 2 minutes to obtain an infrared heat-cured composite board.

7. The use according to claim 6, characterized in that: The infrared light heating device is an infrared lamp with a power of 1000W and a wavelength range of 700-1500nm.

8. The use according to claim 6, characterized in that: In step (3), the pressure to be applied in the cold pressing is 80 psi to 500 psi.

9. The use according to claim 6, characterized in that: The wooden board A and wooden board B are hardwood plywood, softwood plywood, particle board, medium density fiberboard, oriented strand board, waffle board, fiberboard, parallel plywood, shavings laminated timber or hardwood veneer products respectively.