Binder, aqueous metal ion battery negative electrode, aqueous metal ion battery and preparation method

By using a binder with a polysaccharide structure and acrylamide structure on the surface of the negative electrode of the zinc powder, hydrogen evolution, corrosion and dendrite problems in aqueous zinc ion batteries are solved, and the cycle stability and performance of the electrode are improved.

CN119019960APending Publication Date: 2024-11-26SHENZHEN INST OF ADVANCED TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995652.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In aqueous zinc-ion batteries, zinc powder negative electrode materials are prone to side reactions such as hydrogen evolution, corrosion and dendrite in water environments, resulting in poor circulation stability and existing binders cannot effectively suppress these problems.

Method used

Using a binder containing a polymer containing polysaccharide structure and acrylamide structural monomer, it adopts chemical bonds to adsorb the surface of metal powder to form a protective layer, reduces the probability of free water molecules in the electrolyte, inhibits hydrogen evolution and corrosion reactions, and passes through functional groups Guide the metal ion flow to be evenly distributed to prevent dendrites from being produced.

Benefits of technology

The long cycle stability of the zinc powder negative electrode is improved, the passivation layer generation and the reduction of the metal active material quality is reduced, the hydrogen evolution and corrosion side reactions are significantly suppressed, and the stability of the electrode is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019960A_ABST
    Figure CN119019960A_ABST
Patent Text Reader

Abstract

According to the binder, a binder system containing a polysaccharide structure and an acrylamide structure is provided, a protective layer can be formed on the surface of metal powder based on chemical bond adsorption, the protective layer has a hydrophobic chain, the reaction probability of free water molecules in an electrolyte and metal can be reduced, the hydrogen evolution reaction and corrosion side reaction of the metal can be inhibited, and the service life of the metal can be prolonged. Generation of a passivation layer and reduction of the mass of metal powder active matter are reduced; the binder system contains functional groups, and electron-rich functional groups can guide metal ion flow to be uniformly distributed, so that non-uniform deposition of metal is prevented, and generation of metal dendrites is inhibited; the binder provided by the invention can be applied to a metal ion negative electrode system, and can realize relatively high long cycle stability. In addition, the invention also provides an aqueous metal ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal ion batteries, and in particular to a binder, an aqueous metal ion battery negative electrode, an aqueous metal ion battery and a preparation method thereof. Background Art

[0002] Traditional fossil energy resources are limited, and the gases produced during use can cause serious pollution problems. Faced with this situation, we must accelerate the development of new renewable energy sources, such as wind energy, tidal energy, solar energy, etc., to achieve sustainable energy development and ecological environmental protection. However, renewable energy sources such as tidal energy, wind energy and solar energy are extremely dependent on geographical and meteorological environments, and have certain intermittent and volatile characteristics, which brings certain uncertainties to energy supply. Electrochemical energy storage systems can solve these problems. At present, the most widely commercialized battery system is lithium-ion battery, which has been widely used in fields such as mobile devices and electric vehicles due to its high energy density and long cycle life. However, due to the influence of the battery system, lithium-ion batteries are prone to organic electrolyte combustion, fire and even explosion when encountering battery heat release and external impact friction. In addition, during the battery recycling process, the toxicity of organic electrolytes will also have a certain impact on the environment. Therefore, the development of new battery systems is of great significance for environmental protection and sustainable development.

[0003] Aqueous zinc-ion batteries have a high theoretical capacity (820 mAh g -1 ), extremely high safety performance in aqueous environments, and lower cost compared to lithium-ion batteries. It is considered by the scientific research community and industry to be a highly promising next-generation large-scale energy storage chemical battery. Zinc foil, as the negative electrode material of aqueous zinc-ion batteries, will have side reactions such as hydrogen evolution and corrosion to form a passivation layer in an aqueous environment due to its active amphoteric metal properties. In addition, zinc deposition / stripping during battery charging and discharging is prone to form dendrites. Therefore, in order to make aqueous zinc-ion batteries have long-term cycle stability, the above problems must be solved. Compared with zinc foil, zinc powder is easier to process, has lower cost, and has a high utilization rate. It is one of the candidates to replace zinc foil as the negative electrode material of aqueous metal ion batteries. However, its relatively large specific surface area, more serious corrosion, gas production, dendrites and other problems hinder its use as a negative electrode material in aqueous zinc-ion batteries.

[0004] For the problems faced by zinc powder negative electrodes, researchers have proposed some solutions, including coating technology, alloying strategies, selecting different types of conductive carbon, and developing new binders to inhibit side reactions such as hydrogen evolution and dendrites in zinc powder. However, due to the low melting point of zinc metal, coating protection at high temperatures may cause the zinc powder to melt, thereby affecting the coating effect and making it difficult to accurately control the thickness and composition of the protective layer. In addition, although the use of porous carbon as conductive carbon can enhance the electrical contact of the zinc powder negative electrode and reduce the polarization of the zinc powder negative electrode, its high cost will undoubtedly increase the preparation cost of the zinc powder negative electrode. Summary of the invention

[0005] In view of this, it is necessary to provide a binder that can effectively inhibit the hydrogen evolution reaction, enhance the viscosity of the binder and simultaneously improve the transmission efficiency of electrons and ions in order to address the problem that the current binder cannot alleviate the serious side reactions of zinc powder (passivation reaction, hydrogen evolution reaction, etc.).

[0006] To solve the above problems, this application adopts the following technical solutions:

[0007] One of the purposes of the present application is to provide a binder, comprising a polymer containing a polysaccharide structure and a monomer containing an acrylamide structure, wherein:

[0008] The polymer containing a polysaccharide structure includes at least one of sodium carboxymethyl cellulose, sodium alginate, guar gum, gum arabic, modified starch, and chitosan, and the acrylamide structural monomer includes at least one of acrylamide, N-(hydroxymethyl)acrylamide, diacetone acrylamide, N-(isobutyloxy)methyl acrylamide, and N-tert-butyl acrylamide.

[0009] In some embodiments, the mass ratio of the polymer containing a polysaccharide structure to the monomer containing an acrylamide structure is (0.1-1):1.

[0010] The second object of the present application is to provide a method for preparing the adhesive, comprising the following steps:

[0011] The alcohol solution of the polymer containing the polysaccharide structure and the monomer containing the acrylamide structure are mixed and stirred in deionized water to obtain the binder solution.

[0012] In some embodiments, the alcohol solution is added in an amount of 15-60% by mass.

[0013] In some embodiments, the alcohol solution includes at least one of ethanol, methanol, ethylene glycol, propylene glycol, and isopropanol.

[0014] The third object of the present application is to provide a method for preparing a negative electrode of an aqueous metal ion battery using the binder, comprising the following steps:

[0015] Mixing and stirring a solution containing 80% to 90% by mass of metal powder, 5% to 10% of conductive carbon material and the binder to obtain a first mixed solution, wherein the metal powder includes zinc powder, lithium powder, sodium powder, calcium powder, potassium powder or aluminum powder;

[0016] Mixing 0.3%-0.6% by weight of a cross-linking agent, 0.15%-0.3% by weight of an initiator, and the first mixed solution with stirring to obtain a second mixed solution;

[0017] The second mixed solution is coated on the current collector and dried to obtain the aqueous metal ion battery negative electrode.

[0018] In some embodiments, the mesh size of the zinc powder is 200-1500.

[0019] In some embodiments, the conductive carbon material is at least one of carbon nanotubes, acetylene black, Ketjen black, and Super P.

[0020] In some embodiments, the temperature for mixing and stirring the metal powder, the conductive carbon material and the binder solution is 20-40°C.

[0021] In some embodiments, the crosslinking agent is at least one of N,N'-methylenebisacrylamide, divinylbenzene, and diisocyanate.

[0022] In some embodiments, the initiator is at least one of ammonium persulfate, potassium persulfate, sodium persulfate, and sodium perbromide.

[0023] In some of the embodiments, the current collector is not limited to at least one of tinned copper mesh, titanium foil, carbon fiber cloth, graphite paper, and zinc foam.

[0024] In some embodiments, the drying temperature is 60-100°C.

[0025] The fourth object of the present application is to provide an aqueous metal ion battery negative electrode, which is prepared by any of the methods for preparing an aqueous metal ion battery negative electrode.

[0026] The fifth object of the present application is to provide an aqueous metal ion battery, comprising the aqueous metal ion battery negative electrode.

[0027] This application adopts the above technical solution, and its beneficial effects are as follows:

[0028] The binder provided by the present application contains a binder system with a polysaccharide structure and an acrylamide structure. Based on chemical bond adsorption, a protective layer can be formed on the surface of the metal powder. The protective layer has a hydrophobic chain, which can reduce the probability of free water molecules in the electrolyte reacting with the metal, inhibit the hydrogen evolution reaction and corrosion side reactions of the metal, reduce the formation of the passivation layer and the reduction in the amount of active substances in the metal powder; the binder system contains functional groups, and the electron-rich functional groups can guide the uniform distribution of metal ion flow, prevent uneven metal deposition, and inhibit the formation of metal dendrites; the binder provided by the present application can be used in a metal ion negative electrode system to achieve higher long-cycle stability.

[0029] In addition, the raw materials of the binder and aqueous metal ion battery negative electrode provided in this application have significant advantages such as abundant sources, environmental friendliness, low price, and simple preparation method, which are conducive to promoting the further development of aqueous metal ion battery negative electrodes. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0031] Figure 1 It is the X-ray photoelectron spectrum (N1s) of the zinc powder negative electrode under the ratio of Example 1 and the process of Example 5.

[0032] Figure 2 It is the X-ray photoelectron spectrum (O1s) of the zinc powder negative electrode under the ratio of Example 1 and the process of Example 5.

[0033] Figure 3 The linear sweep voltammetry test curve of the electrode obtained in Examples 3 and 4 is shown.

[0034] Figure 4 It is the Tafel curve diagram of the electrode obtained in Examples 3 and 4.

[0035] Figure 5 This is a graph of the zinc-zinc symmetric buckling long cycle performance of the electrode pieces obtained in Examples 3 and 4. DETAILED DESCRIPTION

[0036] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.

[0037] In the description of the present application, it should be understood that the terms "upper", "lower", "horizontal", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0038] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0039] In order to make the objectives, technical solutions and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0040] An adhesive provided in one embodiment of the present application includes a polymer containing a polysaccharide structure and a monomer containing an acrylamide structure.

[0041] The polymer containing a polysaccharide structure includes at least one of sodium carboxymethyl cellulose, sodium alginate, guar gum, gum arabic, modified starch and chitosan.

[0042] It can be understood that the degree of polymerization, number of functional groups and distribution form of the polysaccharide structure of the polymer containing the polysaccharide structure can be adjusted to achieve high bonding performance, thereby increasing the bonding between electrode materials and between the electrode materials and the current collector, regulating the zinc ion nucleation and growth process, reducing the generation of zinc dendrites, and improving the long-cycle stability of the zinc powder negative electrode.

[0043] The acrylamide structural monomer includes at least one of acrylamide, N-(hydroxymethyl)acrylamide, diacetone acrylamide, N-(isobutyloxy)methacrylamide and N-tert-butylacrylamide.

[0044] It can be understood that the acrylamide structural monomer can be polymerized with the polysaccharide structural polymer to form a polymer network structure, and can play a curing role to prevent the electrode from powdering.

[0045] In this embodiment, the mass ratio of the polymer containing a polysaccharide structure to the monomer containing an acrylamide structure is (0.1-1):1.

[0046] It can be understood that, in practice, the composition of the binder can be adjusted according to actual conditions to better meet application requirements.

[0047] Another embodiment of the present application provides a method for preparing the adhesive, comprising the following steps:

[0048] The alcohol solution of the polymer containing the polysaccharide structure and the monomer containing the acrylamide structure are mixed and stirred in deionized water to obtain the binder solution.

[0049] In this embodiment, the added amount of the alcohol solution is 15-60% by mass.

[0050] In this embodiment, the alcohol solution includes at least one of ethanol, methanol, ethylene glycol, propylene glycol, and isopropanol.

[0051] It should be noted that the alcohol solution selected in this embodiment will not react with the aqueous solution, and the alcohol solution is conducive to dispersing the carbon material and preventing the carbon material from agglomerating during the stirring process.

[0052] The chemical formula structure of the binder provided in the above embodiments of the present application can be referred to as follows:

[0053]

[0054] The binder and preparation method thereof provided in the above-mentioned embodiments of the present application use a binder system containing a polysaccharide structure and an acrylamide structure, which can form a protective layer on the surface of a metal powder based on chemical bond adsorption; the protective layer has a hydrophobic chain, which can reduce the probability of free water molecules in the electrolyte reacting with the metal, inhibit the hydrogen evolution reaction and corrosion side reactions of the metal, reduce the generation of a passivation layer and the reduction in the amount of active substances in the metal powder; the binder system contains functional groups, and the electron-rich functional groups can guide the uniform distribution of metal ion flow, prevent uneven zinc deposition, and inhibit the generation of metal dendrites.

[0055] The binder and preparation method thereof provided in the above embodiments of the present application have significant advantages such as abundant sources of raw materials, environmental friendliness, low price, and simple preparation method, which are conducive to promoting the further development of zinc powder negative electrodes.

[0056] Another embodiment of the present application also provides a method for preparing a negative electrode of an aqueous metal ion battery using the binder, comprising the following steps:

[0057] Step S110: 80%-90% by mass of metal powder, 5%-10% of conductive carbon material and a solution of the binder are mixed and stirred to obtain a first mixed solution, wherein the metal powder includes zinc powder, lithium powder, sodium powder, calcium powder, potassium powder or aluminum powder.

[0058] In this embodiment, the mesh size of the metal powder is 200-1500.

[0059] In this embodiment, the conductive carbon material is at least one of carbon nanotubes, acetylene black, Ketjen black, and Super P.

[0060] In this embodiment, the temperature for mixing and stirring the metal powder, the conductive carbon material and the binder solution is 20-40°C.

[0061] Step S120: 0.3%-0.6% by mass of a cross-linking agent, 0.15%-0.3% by mass of an initiator, and the first mixed solution are mixed and stirred to obtain a second mixed solution.

[0062] In this embodiment, the cross-linking agent is at least one of N,N'-methylenebisacrylamide, divinylbenzene, and diisocyanate.

[0063] In this embodiment, the initiator is at least one of ammonium persulfate, potassium persulfate, sodium persulfate, and sodium perbromide.

[0064] Step S130: coating the second mixed solution on the current collector and performing drying treatment to obtain the aqueous metal ion battery negative electrode.

[0065] In this embodiment, the current collector is not limited to at least one of tinned copper mesh, titanium foil, carbon fiber cloth, graphite paper, and foamed zinc.

[0066] It can be understood that the current collector selected in this embodiment has stable physical and chemical properties, does not participate in the reaction, and can provide good electronic conductivity.

[0067] In this embodiment, the drying temperature is 60-100°C.

[0068] The aqueous metal ion battery negative electrode provided in the above-mentioned embodiment of the present application contains a binder system with a polysaccharide structure and an acrylamide structure. Based on chemical bond adsorption, a protective layer can be formed on the surface of the metal powder. The protective layer has a hydrophobic chain, which can reduce the probability of reaction between free water molecules in the electrolyte and the metal, inhibit the hydrogen evolution reaction and corrosion side reactions of the metal, reduce the formation of the passivation layer and the reduction of the active substance mass of the metal powder; the binder system contains functional groups, and the electron-rich functional groups can guide the uniform distribution of the metal ion flow, prevent uneven metal deposition, and inhibit the formation of metal dendrites; the aqueous metal ion battery negative electrode provided by the present application can achieve higher long-cycle stability.

[0069] In addition, the raw materials of the aqueous metal ion battery negative electrode provided in this application have significant advantages such as abundant sources, environmental friendliness, low price, and simple preparation method, which is conducive to promoting the further development of aqueous metal ion battery negative electrodes.

[0070] It should be noted that by selecting different metal ions, it can be applied to the production of different aqueous ion battery electrodes, including zinc ion batteries, lithium ion batteries, sodium ion batteries, calcium ion batteries, potassium ion batteries, aluminum ion batteries, etc., all of which fall within the scope of protection of this patent.

[0071] The above technical solution of the present application is described in detail below in conjunction with specific embodiments.

[0072] Example 1

[0073] This embodiment 1 provides a method for preparing a solution composed of a binder system containing a polysaccharide structure and an acrylamide structure, comprising the following steps:

[0074] Under room temperature, 0.2 g of sodium carboxymethyl cellulose and 0.3 g of acrylamide were weighed and added to a deionized water solution containing alcohol (mass ratio of 1 g alcohol: 7 g water), and stirring was continued until the solution was clear to obtain a binder aqueous solution A with a uniformly mixed polysaccharide structure and acrylamide structure.

[0075] Example 2

[0076] This embodiment 2 provides a method for preparing a solution composed of a binder system containing a polysaccharide structure and an acrylamide structure, comprising the following steps:

[0077] The difference from Example 1 is that the total mass of the polysaccharide structure polymer and the acrylamide structure monomer accounts for a different proportion of the electrode. In Example 2, 0.4g of sodium carboxymethyl cellulose and 0.6g of acrylamide are weighed and added to a deionized water solution containing alcohol (mass ratio is 1g alcohol: 7g water), and stirring is continued until the solution is clear to obtain a uniformly mixed polysaccharide structure and acrylamide structure binder aqueous solution A.

[0078] Example 3

[0079] This embodiment 2 provides a method for preparing a solution composed of a binder system containing a polysaccharide structure and an acrylamide structure, comprising the following steps:

[0080] The difference from Example 1 is that the total mass of the polysaccharide structure polymer and the acrylamide structure monomer accounts for a different proportion of the electrode. In Example 3, 0.1g of sodium alginate and 1g of N-(hydroxymethyl)acrylamide are weighed, added to a deionized water solution containing alcohol (mass ratio of 1g alcohol: 7g water), and stirred continuously until the solution is clear to obtain a uniformly mixed polysaccharide structure and acrylamide structure binder aqueous solution.

[0081] Example 4

[0082] This embodiment 2 provides a method for preparing a solution composed of a binder system containing a polysaccharide structure and an acrylamide structure, comprising the following steps:

[0083] The difference from Example 1 is that the total mass of the polysaccharide structure polymer and the acrylamide structure monomer accounts for a different proportion of the electrode. In Example 3, 1g of guar gum and 1g of diacetone acrylamide are weighed, added to a deionized water solution containing alcohol (mass ratio is 1g alcohol: 7g water), and stirred continuously until the solution is clear to obtain a uniformly mixed polysaccharide structure and acrylamide structure binder aqueous solution.

[0084] Example 5

[0085] This embodiment 5 provides a method for preparing a zinc powder negative electrode, comprising the following steps:

[0086] 9g of zinc powder and 0.5g of Super P were evenly ground in a mortar, added to the binder solution A, and stirred at 25°C for 10min, with a stirring speed of 2000rpm; 0.03g of N,N'-methylenebisacrylamide and 0.003g of ammonium persulfate were added to solution A, and quickly stirred to obtain solution B, which was then evenly applied on a tin-plated copper mesh and dried at 60°C for 2h to obtain a zinc powder negative electrode for an aqueous zinc ion battery. This electrode sheet was an experimental sample, and the weight ratio of the zinc powder active substance, conductive carbon and binder was 90:5:5, and the active substance loading per unit area was 20-24mg.

[0087] Example 6

[0088] This embodiment 6 provides a method for preparing a zinc powder negative electrode containing a commercial binder system, comprising the following steps:

[0089] The difference from Example 5 is that the added binder is a commercial polytetrafluoroethylene binder. In Example 6, 9g of zinc powder and 0.5g of Super P were uniformly mixed in a mortar, ground for 5 minutes, 0.5g of polytetrafluoroethylene (PTFE) was added to the mortar, ethanol was slowly added and repeatedly pressed, and then pressed on a tinned copper mesh. The prepared pole piece is a comparative sample, and the weight ratio of the zinc powder active material, conductive carbon and binder is 90:5:5, and the active material loading per unit area is 20-30mg.

[0090] Example 7

[0091] This Example 7 provides a test of a binder containing a polysaccharide structure and an acrylamide structure on the surface interface layer of a zinc powder negative electrode:

[0092] The zinc powder negative electrode was prepared under the operation of Example 7, and the chemical composition of its interface layer was characterized by X-ray photoelectron spectroscopy, such as Figure 1 As shown, the N 1s X-ray photoelectron spectrum shows that there is a strong nitrogen-zinc bond peak on the surface of the zinc powder, indicating that the amide group in acrylamide is adsorbed on the surface of the zinc powder.

[0093] like Figure 2 The O1s X-ray photoelectron spectrum shown in the figure shows that there is a strong oxygen-zinc bond peak on the surface of the zinc powder, indicating that the carboxyl groups in the sodium carboxymethyl cellulose are adsorbed on the surface of the zinc powder.

[0094] Example 8

[0095] This Example 8 provides a test of the anti-hydrogen evolution performance of zinc powder negative electrode by a binder containing a polysaccharide structure and an acrylamide structure:

[0096] Then, the experimental sample prepared in Example 5 and the comparative sample prepared in Example 6 were cut into circular electrodes with a diameter of 12 mm as working electrodes, foils as counter electrodes, and saturated silver chloride as reference electrodes to form a three-electrode system, and the three-electrode system was tested by linear scanning voltammetry using an electrochemical workstation.

[0097] like Figure 3 As shown, compared with the control sample, the scanning voltage of the experimental sample is from -1.15V to -1.8V, and the hydrogen evolution current is moved from 50mV to 20mV, indicating that the binder of the experimental sample can effectively inhibit the hydrogen evolution side reaction of zinc powder.

[0098] Example 9

[0099] This Example 9 provides a test of the corrosion resistance of a zinc powder negative electrode by a binder containing a polysaccharide structure and an acrylamide structure:

[0100] Then, the experimental sample prepared in Example 5 and the comparative sample prepared in Example 6 were cut into circular electrodes with a diameter of 12 mm as working electrodes, foils as counter electrodes, and saturated silver chloride as reference electrodes to form a three-electrode system, and Tafel test was performed on the three-electrode system using an electrochemical workstation.

[0101] like Figure 4 As shown in the figure, the corrosion current of the experimental sample decreased from 4.4 mA to 1.1 mA compared with the control sample, which indicates that the binder of the experimental sample can effectively inhibit the corrosion side reaction of zinc powder.

[0102] Example 10

[0103] This embodiment provides a binder containing a polysaccharide structure and an acrylamide structure for zinc powder negative electrode symmetric battery assembly and long cycle testing:

[0104] (1) Battery assembly: For the experimental zinc-zinc symmetrical battery, the anode and cathode are both made of the electrode sheets in Example 5; for the comparative zinc-zinc symmetrical battery, the positive electrode and negative electrode are both made of the electrode sheets in Example 4. The assembled battery is a button battery, and its structure is a negative electrode shell, a spring sheet, a gasket, a negative electrode, a diaphragm, a positive electrode, and a positive electrode shell.

[0105] (2) Electrochemical test: At room temperature, the assembled zinc-zinc symmetric button cell was charged and discharged on a Xinwei battery test system at a current density of 5 mA / cm 2 , deposition capacity is 5 mAh / cm 2 , its cycle performance is as follows Figure 5 As shown, under this condition, the experimental sample can be stably cycled symmetrically for 1200 hours.

[0106] It can be understood that the technical features of the above-described embodiments can be arbitrarily combined. In order to make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0107] The above are only preferred embodiments of the present application, and only specifically describe the technical principles of the present application. These descriptions are only for explaining the principles of the present application and cannot be interpreted as limiting the scope of protection of the present application in any way. Based on the explanation here, any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application, and other specific implementation methods of the present application that can be associated with the technicians in this field without creative work, should be included in the scope of protection of the present application.

Claims

1. A binder, characterized in that: It includes polymers containing polysaccharide structures and monomers containing acrylamide structures, wherein: The polymer containing a polysaccharide structure includes at least one of sodium carboxymethyl cellulose, sodium alginate, guar gum, gum arabic, modified starch, and chitosan, and the acrylamide structural monomer includes at least one of acrylamide, N-(hydroxymethyl)acrylamide, diacetone acrylamide, N-(isobutyloxy)methyl acrylamide, and N-tert-butyl acrylamide.

2. The adhesive according to claim 1, characterized in that The mass ratio of the polymer containing a polysaccharide structure to the monomer containing an acrylamide structure is (0.1-1):

1.

3. A method for preparing the adhesive according to claim 1, characterized in that: The steps include: The alcohol solution of the polymer containing the polysaccharide structure and the monomer containing the acrylamide structure are mixed and stirred in deionized water to obtain the binder solution.

4. The method for preparing the adhesive according to claim 3, characterized in that: The added amount of the alcohol solution is 15-60% by mass.

5. The method for preparing the adhesive according to claim 3, characterized in that: The alcohol solution includes at least one of ethanol, methanol, ethylene glycol, propylene glycol, and isopropanol.

6. A method for preparing an aqueous metal ion battery negative electrode comprising the binder according to claim 3, characterized in that: The steps include: Mixing and stirring 80%-90% by mass of metal powder, 5%-10% of conductive carbon material and a solution of the binder to obtain a first mixed solution, wherein the metal powder includes zinc powder, lithium powder, sodium powder, calcium powder, potassium powder or aluminum powder; Mixing and stirring 0.3%-0.6% by weight of a cross-linking agent, 0.15%-0.3% by weight of an initiator, and the first mixed solution to obtain a second mixed solution; The second mixed solution is coated on the current collector and dried to obtain the aqueous metal ion battery negative electrode.

7. The method for preparing the negative electrode of an aqueous metal ion battery according to claim 6, characterized in that: The mesh number of the metal powder is 200-1500.

8. The method for preparing the negative electrode of an aqueous metal ion battery according to claim 6, characterized in that: The conductive carbon material is at least one of carbon nanotubes, acetylene black, Ketjen black and Super P.

9. The method for preparing the negative electrode of an aqueous metal ion battery according to claim 6, characterized in that: The temperature for mixing and stirring the metal powder, the conductive carbon material and the binder solution is 20-40°C.

10. The method for preparing the negative electrode of an aqueous metal ion battery according to claim 6, characterized in that: The crosslinking agent is at least one of N,N'-methylenebisacrylamide, divinylbenzene and diisocyanate.

11. The method for preparing the negative electrode of an aqueous metal ion battery according to claim 6, characterized in that: The initiator is at least one of ammonium persulfate, potassium persulfate, sodium persulfate and sodium perbromide.

12. The method for preparing the negative electrode of an aqueous metal ion battery according to claim 6, characterized in that: The current collector is not limited to at least one of tinned copper mesh, titanium foil, carbon fiber cloth, graphite paper, and zinc foam.

13. The method for preparing the negative electrode of an aqueous metal ion battery according to claim 6, characterized in that: The drying temperature is 60-100°C.

14. A negative electrode for an aqueous metal ion battery, characterized in that: The negative electrode of an aqueous metal ion battery is prepared by the method for preparing the negative electrode of an aqueous metal ion battery according to any one of claims 1 to 13.