High-strength high-elasticity polyether modified epoxy structural adhesive and preparation method thereof

By synthesizing a silicone-modified epoxy curing agent and using it in combination with epoxy resin and silane-modified polyether, the strength and elasticity of epoxy structural adhesives were improved, solving the dynamic durability problem of epoxy adhesives in the fields of new energy vehicles and transportation, and achieving high strength and high elasticity.

CN119019969APending Publication Date: 2024-11-26GUANGZHOU BAIYUN CHEM IND +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411116200.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing epoxy adhesives are too rigid and lack elasticity in the fields of new energy vehicles and transportation, resulting in poor dynamic durability and making it difficult to meet the performance requirements of high-elasticity structural adhesives.

Method used

Organosilicon-modified epoxy curing agents were synthesized by reacting γ-glycidyl etheroxypropyltrimethoxysilane with polyetheramine, and then used in combination with epoxy resin and silane-modified polyether to improve the strength and elasticity of structural adhesives.

Benefits of technology

The prepared high-strength, high-elasticity polyether-modified epoxy structural adhesive has a shear strength greater than 8 MPa, a tensile strength greater than 7 MPa, and an elongation at break greater than 300%, exhibiting excellent waterproof and sealing properties, and is suitable for new energy vehicles and transportation applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993685230000011
    Figure BDA0004993685230000011
  • Figure BDA0004993685230000021
    Figure BDA0004993685230000021
  • Figure BDA0004993685230000022
    Figure BDA0004993685230000022
Patent Text Reader

Abstract

The invention belongs to the technical field of structural adhesives, and discloses a high-strength high-elasticity polyether modified epoxy structural adhesive which comprises a component A and a component B, the component A is prepared from the following raw materials in parts by weight: 15-60 parts of a silane modified polyether polymer, 5-40 parts of a plasticizer, 10-50 parts of a filler A, 1-5 parts of a thixotropic agent, 1-5 parts of a silane coupling agent and 5-35 parts of an organic silicon modified epoxy curing agent; the component B is prepared from the following raw materials in parts by weight: 20-60 parts of epoxy resin, 10-40 parts of a reactive diluent, 15-50 parts of a filler B and 0.5-5 parts of an organic tin catalyst; wherein the organic silicon modified epoxy curing agent is obtained by carrying out a reaction on gamma-glycidyl ether oxypropyl trimethoxy silane and polyether amine. The high-strength and high-elasticity polyether modified epoxy structural adhesive has excellent strength and elasticity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of structural adhesives, and in particular relates to a high-strength and high-elasticity polyether-modified epoxy structural adhesive and a preparation method thereof. Background Art

[0002] Epoxy adhesives have the advantages of high bonding strength, good chemical resistance, and a wide range of applications. They are often used as structural adhesives in the fields of new energy vehicles, transportation, etc. However, epoxy adhesives are often too rigid and lack elasticity, and are prone to brittle fracture. In application fields such as new energy vehicles and transportation that are often in motion, the lack of elasticity of structural adhesives will affect their dynamic durability. Especially in the newly emerging new energy vehicle power battery FDS glue-riveted combined box in recent years, the adhesive is required to have good elasticity (usually the elongation at break is required to be greater than 200%) while playing a structural bonding role, in order to improve dynamic durability and achieve a good waterproof sealing effect. Therefore, it is very necessary to study a high-strength and high-elasticity epoxy structural adhesive.

[0003] Epoxy adhesive is a commonly used structural adhesive. It is very rigid. Modification with toughening agent is an important means to improve its elasticity. However, the elongation at break of epoxy adhesive modified with common toughening agent is usually difficult to exceed 100%, which is difficult to meet the performance requirements of high elastic structural adhesive for the FDS glue-riveted bonding box of power batteries. Silane-modified polyether adhesive is an elastic adhesive with very good elasticity. However, its strength is not very high, and it is insufficient for use as a structural adhesive. Summary of the invention

[0004] The object of the present invention is to provide a high-strength and high-elasticity polyether-modified epoxy structural adhesive, which has both excellent strength and elasticity properties.

[0005] The above-mentioned purpose is achieved by the following technical solutions.

[0006] A first aspect of an embodiment of the present invention provides a high-strength and high-elasticity polyether-modified epoxy structural adhesive, comprising a component A and a component B;

[0007] The A component is made of the following raw materials in parts by weight:

[0008]

[0009]

[0010] The B component is made of the following raw materials in parts by weight:

[0011]

[0012] The organosilicon-modified epoxy curing agent is obtained by reacting γ-glycidyloxypropyltrimethoxysilane and polyetheramine.

[0013] In some embodiments, the A component is made of raw materials including the following components in parts by weight:

[0014]

[0015] The B component is made of the following raw materials in parts by weight:

[0016]

[0017] The A component is made of the following raw materials in parts by weight:

[0018]

[0019]

[0020] The B component is made of the following raw materials in parts by weight:

[0021]

[0022] In some embodiments, the organosilicon-modified epoxy curing agent has the following structure:

[0023]

[0024] Wherein, n is any integer of 2, 3, 4, 5, and 6.

[0025] In some embodiments, the polyetheramine has the following structure:

[0026]

[0027] Wherein, n is any integer of 2, 3, 4, 5, and 6.

[0028] In some embodiments, the molar ratio of γ-glycidyloxypropyltrimethoxysilane to polyetheramine is 1:1-1.2; and / or,

[0029] The preparation method of the organosilicon-modified epoxy curing agent comprises the following steps:

[0030] At a temperature of 25°C to 80°C, γ-glycidyloxypropyltrimethoxysilane is added dropwise to the polyetheramine while stirring, and then stirred for 10min to 30min after the addition is complete to obtain the organosilicon-modified epoxy curing agent, and the reaction formula is as follows:

[0031]

[0032] In some embodiments, the silane-modified polyether polymer in component A is at least one of a dimethoxy-terminated silane-modified polyether polymer and a trimethoxy-terminated silane-modified polyether polymer; preferably, the viscosity of the silane-modified polyether polymer at 25° C. is 6 Pa.s to 82 Pa.s.

[0033] In some embodiments, the plasticizer includes at least one of dioctyl phthalate, diisodecyl phthalate, diisononyl phthalate, dibutyl phthalate, dioctyl adipate, diisodecyl adipate, dioctyl sebacate, diisooctyl sebacate, diphenyl octyl phosphate, diphenyl diphenyl phosphate and polypropylene glycol; and / or,

[0034] The filler A comprises at least one of nano calcium carbonate, heavy calcium carbonate, silicon powder, nano fumed silica, alumina, aluminum hydroxide, talc and carbon black; and / or,

[0035] The thixotropic agent includes at least one of polyamide wax, hydrogenated castor oil and organic bentonite; and / or,

[0036] The silane coupling agent includes at least one of acryloxypropyltrimethoxysilane, 2-cyanoethyltriethoxysilane, γ-mercaptopropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, N,N-dimethyl-3-aminopropyltrimethoxysilane, N-n-butyl-3-aminopropyltriethoxysilane, and 3-(diethylenetriamino)propyltrimethoxysilane.

[0037] In some embodiments, the epoxy resin includes at least one of bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, castor oil modified epoxy resin, polyurethane modified epoxy resin, silicone modified epoxy resin, and acrylate modified epoxy resin; and / or,

[0038] The active diluent includes at least one of 1,4-butanediol diglycidyl ether, dodecyl glycidyl ether, benzyl glycidyl ether, cardanol glycidyl ether, etc.; and / or,

[0039] The filler B includes at least one of nano calcium carbonate, heavy calcium carbonate, silicon powder, fumed silica, alumina, aluminum hydroxide, talc, and carbon black; and / or,

[0040] The organic tin catalyst includes at least one of dibutyltin diacetate, dibutyltin dilaurate, dioctyltin diacetate, stannous octoate and di-n-butylbis(acetylacetonato)tin.

[0041] In some embodiments, the volume ratio of the component A to the component B is 1-5:1; preferably, the volume ratio of the component A to the component B is 1-2:1.

[0042] The second aspect of the present invention provides a method for preparing the high-strength and high-elasticity polyether-modified epoxy structural adhesive as described above, comprising the following steps:

[0043] The silane-modified polyether polymer, the plasticizer, the filler A, and the thixotropic agent are mixed and stirred evenly, and then the silane coupling agent and the organosilicon-modified epoxy curing agent are added and mixed and stirred evenly to obtain the component A;

[0044] The epoxy resin, active diluent, filler B and organotin catalyst are mixed and stirred uniformly to obtain component B.

[0045] In the present invention, the inventors synthesized a silicone-modified epoxy curing agent by reacting specific γ-glycidyloxypropyltrimethoxysilane and polyetheramine, and found that the silicone-modified epoxy curing agent has a synergistic effect when used in combination with epoxy resin and silane-modified polyether, and can improve the strength and elastic properties of the structural adhesive, so that the prepared polyether-modified epoxy structural adhesive has both excellent strength and elastic properties, and its shear strength is greater than 8MPa, the tensile strength is greater than 7MPa, and the elongation at break is greater than 300%. It has broad application prospects in the fields of new energy vehicles, transportation, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is the hydrogen spectrum of the organosilicon-modified epoxy curing agent of Example 2 of the present invention.

[0047] Figure 2 This is the infrared spectrum of the organosilicon-modified epoxy curing agent of Example 2 of the present invention. DETAILED DESCRIPTION

[0048] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0049] The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or conditions recommended by the manufacturers. The various commonly used chemical reagents used in the examples are all commercially available products.

[0050] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.

[0051] Example 1

[0052] The high-strength and high-elasticity polyether-modified epoxy structural adhesive provided in this embodiment is prepared from the following components in parts by weight:

[0053] Component A:

[0054]

[0055] Component B contains:

[0056]

[0057] The structural formula of the silane-modified polyether polymer in the A component is:

[0058] Its viscosity at 25°C is 20 pa.s;

[0059] The preparation process of the organosilicon-modified epoxy curing agent is as follows: firstly, a certain amount of polyetheramine is added into a reaction container with heating and stirring, then the temperature is raised to 50°C, and γ-glycidyloxypropyltrimethoxysilane is added dropwise while stirring [the molar ratio of γ-glycidyloxypropyltrimethoxysilane to polyetheramine is 1:1], and the organosilicon-modified epoxy curing agent is obtained by stirring for 20 minutes after the addition is completed.

[0060] The reaction formula is as follows:

[0061]

[0062] The structural formula of the obtained organosilicon-modified epoxy curing agent is:

[0063]

[0064] n=3.

[0065] The silane-modified polyether polymer, PPG3000, nano-calcium carbonate and polyamide wax are mixed and stirred evenly, and then acryloxypropyltrimethoxysilane and silicone-modified epoxy curing agent are added and mixed and stirred evenly to obtain the component A.

[0066] Bisphenol A diglycidyl ether E51, 1,4-butanediol diglycidyl ether, nano-fumed silica and dibutyltin dilaurate are mixed and stirred uniformly to obtain component B.

[0067] When using, press A:B=2:1 (volume ratio) and mix evenly.

[0068] Example 2

[0069] The high-strength and high-elasticity polyether-modified epoxy structural adhesive provided in this embodiment is prepared from the following components in parts by weight:

[0070] Component A:

[0071]

[0072] Component B contains:

[0073]

[0074]

[0075] The structural formula of the silane-modified polyether polymer in the A component is:

[0076] Its viscosity at 25°C is 20 pa.s;

[0077] The preparation process of the organosilicon-modified epoxy curing agent is as follows: firstly, a certain amount of polyetheramine is added into a reaction container with heating and stirring, then the temperature is raised to 60° C., and γ-glycidyloxypropyltrimethoxysilane is added dropwise while stirring [the molar ratio of γ-glycidyloxypropyltrimethoxysilane to polyetheramine is 1:1.15], and the organosilicon-modified epoxy curing agent is obtained by stirring for 10 minutes after the addition is completed.

[0078] The structural formula of the obtained organosilicon-modified epoxy curing agent is:

[0079]

[0080] n=2.

[0081] in Figure 1This is the hydrogen spectrum of the obtained silicone-modified epoxy curing agent. From the hydrogen spectrum, it can be seen that the relatively weak proton peak at the chemical shift δ=7.72ppm belongs to the peak of the secondary amine group. The chemical shift δ=6.01ppm is the OH proton peak next to the secondary amine group. The chemical shift δ=4.93ppm is the methylene CH proton peak connected to OH. The relatively strong peak at the chemical shift δ=3.55ppm is the proton peak of the three CH3-O. The relatively broad peak near δ=3.35ppm should be attributed to the proton peak of CH2. The methylene CH proton peak appears near δ=2.93ppm. The relatively strong proton peak at δ=1.06ppm is attributed to the proton peak of CH3 near the primary amine.

[0082] Figure 2 This is the infrared spectrum of the obtained organosilicon-modified epoxy curing agent. It can be seen from the infrared spectrum that there is an obvious infrared characteristic absorption peak of epoxy group at 910cm-1 in γ-glycidyloxypropyltrimethoxysilane; there is an obvious NH infrared absorption peak at 3367cm-1 in polyetheramine; in the modified curing agent, the infrared peak at 910cm-1 almost disappears, proving that the epoxy group is almost consumed, while there is still an obvious NH absorption peak at 3416cm-1, indicating that an organosilicon-modified epoxy curing agent is obtained.

[0083] The silane-modified polyether polymer, dioctyl phthalate, nano-fumed silica and hydrogenated castor oil are mixed and stirred evenly, and then 2-cyanoethyl triethoxysilane and organosilicon-modified epoxy curing agent are added and mixed and stirred evenly to obtain component A.

[0084] Bisphenol F diglycidyl ether, dodecyl glycidyl ether, nano calcium carbonate and dibutyltin diacetate are mixed and stirred uniformly to obtain component B.

[0085] When using, press A:B=2:1 (volume ratio) and mix evenly.

[0086] Example 3

[0087] The high-strength and high-elasticity polyether-modified epoxy structural adhesive provided in this embodiment is prepared from the following components in parts by weight:

[0088] Component A:

[0089]

[0090] Component B contains:

[0091]

[0092] The structural formula of the silane-modified polyether polymer in the A component is:

[0093] Its viscosity at 25°C is 20 pa.s;

[0094] The preparation method of the organosilicon-modified epoxy curing agent is consistent with that of Example 2. The structural formula of the prepared organosilicon-modified epoxy curing agent is:

[0095]

[0096] n=2.

[0097] The silane-modified polyether polymer, dioctyl phthalate, nano-fumed silica and polyamide wax are mixed and stirred evenly, and then acryloxypropyltrimethoxysilane and silicone-modified epoxy curing agent are added and mixed and stirred evenly to obtain the component A.

[0098] Bisphenol A diglycidyl ether E51, 1,4-butanediol diglycidyl ether, nano-fumed silica and dibutyltin dilaurate are mixed and stirred uniformly to obtain component B.

[0099] When using, press A:B=2:1 (volume ratio) and mix evenly.

[0100] Example 4

[0101] The high-strength and high-elasticity polyether-modified epoxy structural adhesive provided in this embodiment is prepared from the following components in parts by weight:

[0102] Component A:

[0103]

[0104] Component B contains:

[0105]

[0106] The structural formula of the silane-modified polyether polymer in the A component is:

[0107] Its viscosity at 25°C is 30pa.s;

[0108] The preparation process of the organosilicon-modified epoxy curing agent is as follows: firstly, a certain amount of polyetheramine is added into a reaction container with heating and stirring, and then, at 25°C, γ-glycidyloxypropyltrimethoxysilane [γ-glycidyloxypropyltrimethoxysilane) and polyetheramine are added dropwise while stirring in a molar ratio of 1:1.2], and after the addition is completed, the mixture is stirred for 30 minutes to obtain the organosilicon-modified epoxy curing agent.

[0109] The structural formula of the obtained organosilicon-modified epoxy curing agent is:

[0110]

[0111] n=6.

[0112] The silane-modified polyether polymer, diisodecyl phthalate, nano-calcium carbonate and organic bentonite are mixed and stirred evenly, and then γ-mercaptopropyl triethoxysilane and organic silicon-modified epoxy curing agent are added and mixed and stirred evenly to obtain the component A.

[0113] The polyurethane modified epoxy resin, benzyl glycidyl ether, nano calcium carbonate and di-n-butyl bis(acetylacetonato)tin are mixed and stirred uniformly to obtain component B.

[0114] When using, press A:B=2:1 (volume ratio) and mix evenly.

[0115] Example 5

[0116] The high-strength and high-elasticity polyether-modified epoxy structural adhesive provided in this embodiment is prepared from the following components in parts by weight:

[0117] Component A:

[0118]

[0119] Component B contains:

[0120]

[0121]

[0122] The structural formula of the silane-modified polyether polymer in the A component is:

[0123] Its viscosity at 25°C is 40pa.s;

[0124] The preparation method of the organosilicon-modified epoxy curing agent is consistent with that of Example 2. The structural formula of the prepared organosilicon-modified epoxy curing agent is:

[0125]

[0126] n=2.

[0127] The silane-modified polyether polymer, PPG2000, nano-fumed silica and polyamide wax are mixed and stirred evenly, and then acryloxypropyltrimethoxysilane and silicone-modified epoxy curing agent are added and mixed and stirred evenly to obtain the component A.

[0128] The polyurethane modified epoxy resin, cardanol glycidyl ether, nano calcium carbonate and di-n-butyl bis(acetylacetonato)tin are mixed and stirred uniformly to obtain component B.

[0129] When using, press A:B=1:1 (volume ratio) and mix evenly.

[0130] Comparative Example 1

[0131] The high-strength and high-elasticity polyether-modified epoxy structural adhesive provided in this comparative example is different from that in Example 1 in that the silane-modified polyether polymer component of component A in Example 1 is removed. It is mainly prepared from the following components in parts by weight:

[0132] Component A:

[0133]

[0134] Component B contains:

[0135] Bisphenol A diglycidyl ether E51 40

[0136] 1,4-Butanediol diglycidyl ether 30

[0137] Nano-fumed silica 30.

[0138] The preparation method of the organosilicon-modified epoxy curing agent is consistent with that in Example 1. The structural formula of the prepared organosilicon-modified epoxy curing agent is:

[0139]

[0140] n=3.

[0141] The nano calcium carbonate and polyamide wax are mixed and stirred evenly, and then acryloxypropyl trimethoxy silane and silicone-modified epoxy curing agent are added and mixed and stirred evenly to obtain the component A.

[0142] Bisphenol A diglycidyl ether E51, 1,4-butanediol diglycidyl ether and nano-fumed silica are mixed and stirred uniformly to obtain component B.

[0143] When using, press A:B=2:1 (volume ratio) and mix evenly.

[0144] Comparative Example 2

[0145] The high-strength and high-elasticity polyether-modified epoxy structural adhesive provided in this comparative example is different from that in Example 1 in that the epoxy resin in the component B of Example 1 is removed, and the other components remain unchanged. It is mainly prepared from the following components in parts by weight:

[0146] Component A:

[0147]

[0148] Component B contains:

[0149] 1,4-Butanediol diglycidyl ether 30

[0150] Nano fumed silica 28

[0151] Dibutyltin dilaurate

[0152] The structural formula of the silane-modified polyether polymer in the A component is:

[0153] Its viscosity at 25°C is 20 pa.s;

[0154] The silane-modified polyether polymer, PPG3000, nano-calcium carbonate and polyamide wax are mixed and stirred evenly, and then acryloxypropyltrimethoxysilane and silicone-modified epoxy curing agent are added and mixed and stirred evenly to obtain the component A.

[0155] 1,4-Butanediol diglycidyl ether, filler B and dibutyltin dilaurate are mixed and stirred uniformly to obtain component B.

[0156] When using, press A:B=2:1 (volume ratio) and mix evenly.

[0157] Comparative Example 3

[0158] The high-strength and high-elasticity polyether-modified epoxy structural adhesive provided in this comparative example is different from Example 1 in that the organosilicon-modified epoxy curing agent is replaced with a polyetheramine curing agent, and the rest remains unchanged. It is mainly prepared from the following components in parts by weight:

[0159] Component A:

[0160]

[0161] Component B contains:

[0162]

[0163] The structural formula of the silane-modified polyether polymer in the A component is:

[0164] Its viscosity at 25°C is 20 pa.s;

[0165] The structural formula of the polyetheramine is:

[0166]

[0167] n=3.

[0168] The silane-modified polyether polymer, PPG3000, nano-calcium carbonate and polyamide wax are mixed and stirred evenly, and then acryloxypropyltrimethoxysilane and polyetheramine are added and mixed and stirred evenly to obtain the component A.

[0169] Mix bisphenol A diglycidyl ether E51, 1,4-butanediol diglycidyl ether, nano-fumed silica, and dibutyltin dilaurate and stir evenly to obtain component B.

[0170] When using, press A:B=2:1 (volume ratio) and mix evenly.

[0171] Comparative Example 4

[0172] The high-strength and high-elasticity polyether-modified epoxy structural adhesive provided in this comparative example is different from Example 1 in that the epoxy resin, active diluent, and curing agent-related components in Example 1 are removed, the active diluent of component B is changed to PPG3000, and the other components remain unchanged. The other components remain unchanged. It is mainly prepared from the following components in parts by weight:

[0173] Component A:

[0174]

[0175] Component B contains:

[0176] PPG3000 30

[0177] Nano fumed silica 28

[0178] Dibutyltin dilaurate

[0179] The structural formula of the silane-modified polyether polymer in the A component is:

[0180] Its viscosity at 25°C is 20 pa.s;

[0181] The silane-modified polyether polymer, PPG3000, nano-calcium carbonate and polyamide wax are mixed and stirred evenly, and then acryloxypropyltrimethoxysilane is added and mixed and stirred evenly to obtain the component A.

[0182] Mix PPG3000, filler B and dibutyltin dilaurate and stir evenly to obtain component B.

[0183] When using, press A:B=2:1 (volume ratio) and mix evenly.

[0184] The structural adhesives prepared in Examples 1-5 and Comparative Examples 1-4 were subjected to the following performance tests:

[0185] Shear strength: Tested according to GB / T 7124 method.

[0186] Tensile strength: Tested according to GB / T 528 method.

[0187] Elongation at break: Tested according to GB / T 528 method.

[0188] Waterproof grade: tested according to GB / T 4208-2017 method.

[0189] The test results are shown in Table 1.

[0190] Table 1 Performance parameters of high-strength and high-elasticity polyether modified epoxy structural adhesive examples

[0191] project Shear strength / MPa Tensile strength / MPa Elongation at break / % Waterproof grade Example 1 8.6 7.9 350 IP68 Example 2 8.1 7.4 380 IP68 Example 3 8.8 8.1 360 IP68 Example 4 8.7 7.9 355 IP68 Example 5 8.2 7.5 320 IP68 Comparative Example 1 15.3 33.5 2 IP67 Comparative Example 2 3.4 4.0 350 IP68 Comparative Example 3 4.6 5.1 260 IP68 Comparative Example 4 2.8 3.0 580 IP68

[0192] It can be seen from the experimental results of Table 1 that the high-strength and high-elasticity epoxy structural adhesives of Examples 1-5 prepared by the synthesized organosilicon-modified epoxy curing agent of the present invention all have relatively high shear strength, tensile strength, elongation at break and waterproof sealing performance. Comparative Example 1 is a simple two-component epoxy structural adhesive, and its elongation at break is very low, indicating that its elasticity is poor. Comparative Example 2, due to the removal of epoxy resin, more shows the characteristics of silane-modified polyether adhesive, which has a higher elongation at break, but its strength is not large. Comparative Example 3 using polyetheramine curing agent, because the polyetheramine epoxy curing agent only reacts with epoxy resin, resulting in the final product strength and elasticity are not very good. Comparative Example 4 is a simple two-component silane-modified polyether adhesive, which has a very high elongation at break, but its strength is not large. In Examples 1-5, the organosilicon-modified polyetheramine epoxy curing agent synthesized by the present invention is used. The organosilicon-modified epoxy curing agent has a synergistic effect when used in combination with epoxy resin and silane-modified polyether, fully demonstrating the advantages of high strength of epoxy adhesive and high elasticity of silane-modified polyether adhesive.

[0193] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0194] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A high-strength and high-elastic polyether-modified epoxy structural adhesive, characterized in that: It includes component A and component B; The A component is made of the following raw materials in parts by weight: The B component is made of the following raw materials in parts by weight: The organosilicon-modified epoxy curing agent is obtained by reacting γ-glycidyloxypropyltrimethoxysilane and polyetheramine.

2. The high-strength and high-elastic polyether-modified epoxy structural adhesive according to claim 1, characterized in that: The A component is made of the following raw materials in parts by weight: The B component is made of the following raw materials in parts by weight: The A component is made of the following raw materials in parts by weight: The B component is made of the following raw materials in parts by weight:

3. The high-strength and high-elastic polyether-modified epoxy structural adhesive according to claim 1, characterized in that: The organosilicon-modified epoxy curing agent has the following structure: Wherein, n is any integer of 2, 3, 4, 5, and 6.

4. The high-strength and high-elastic polyether-modified epoxy structural adhesive according to claim 1, characterized in that: The polyetheramine has the following structure: Wherein, n is any integer of 2, 3, 4, 5, and 6.

5. The high-strength and high-elastic polyether-modified epoxy structural adhesive according to claim 1, characterized in that: The molar ratio of γ-glycidyloxypropyltrimethoxysilane to polyetheramine is 1:1 to 1.2; and / or, The preparation method of the organosilicon-modified epoxy curing agent comprises the following steps: At a temperature of 25°C to 80°C, γ-glycidyloxypropyltrimethoxysilane is added dropwise to the polyetheramine while stirring, and then stirred for 10min to 30min after the addition is complete to obtain the organosilicon-modified epoxy curing agent, and the reaction formula is as follows:

6. The high-strength and high-elastic polyether-modified epoxy structural adhesive according to any one of claims 1 to 5, characterized in that: The silane-modified polyether polymer in the A component is at least one of a dimethoxy-terminated silane-modified polyether polymer and a trimethoxy-terminated silane-modified polyether polymer; preferably, the viscosity of the silane-modified polyether polymer at 25° C. is 6 Pa.s to 82 Pa.s.

7. The high-strength and high-elastic polyether-modified epoxy structural adhesive according to any one of claims 1 to 5, characterized in that: The plasticizer comprises at least one of dioctyl phthalate, diisodecyl phthalate, diisononyl phthalate, dibutyl phthalate, dioctyl adipate, diisodecyl adipate, dioctyl sebacate, diisooctyl sebacate, diphenyl octyl phosphate, diphenyl diphenyl phosphate and polypropylene glycol; and / or, The filler A comprises at least one of nano calcium carbonate, heavy calcium carbonate, silicon powder, nano fumed silica, alumina, aluminum hydroxide, talc and carbon black; and / or, The thixotropic agent includes at least one of polyamide wax, hydrogenated castor oil and organic bentonite; and / or, The silane coupling agent includes at least one of acryloxypropyltrimethoxysilane, 2-cyanoethyltriethoxysilane, γ-mercaptopropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, N,N-dimethyl-3-aminopropyltrimethoxysilane, N-n-butyl-3-aminopropyltriethoxysilane, and 3-(diethylenetriamino)propyltrimethoxysilane.

8. The high-strength and high-elastic polyether-modified epoxy structural adhesive according to any one of claims 1 to 5, characterized in that: The epoxy resin includes at least one of bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, castor oil modified epoxy resin, polyurethane modified epoxy resin, silicone modified epoxy resin, and acrylate modified epoxy resin; and / or, The active diluent includes at least one of 1,4-butanediol diglycidyl ether, dodecyl glycidyl ether, benzyl glycidyl ether, cardanol glycidyl ether, etc.; and / or, The filler B includes at least one of nano calcium carbonate, heavy calcium carbonate, silicon powder, fumed silica, alumina, aluminum hydroxide, talc, and carbon black; and / or, The organic tin catalyst includes at least one of dibutyltin diacetate, dibutyltin dilaurate, dioctyltin diacetate, stannous octoate and di-n-butylbis(acetylacetonato)tin.

9. The high-strength and high-elastic polyether-modified epoxy structural adhesive according to any one of claims 1 to 5, characterized in that: The volume ratio of the component A to the component B is 1 to 5:1; preferably, the volume ratio of the component A to the component B is 1 to 2:

1.

10. A method for preparing the high-strength and high-elastic polyether-modified epoxy structural adhesive according to any one of claims 1 to 9, characterized in that: The steps include: The silane-modified polyether polymer, the plasticizer, the filler A, and the thixotropic agent are mixed and stirred evenly, and then the silane coupling agent and the organosilicon-modified epoxy curing agent are added and mixed and stirred evenly to obtain the component A; The epoxy resin, active diluent, filler B and organotin catalyst are mixed and stirred uniformly to obtain component B.

Citation Information

Cited By

  • Long-acting mildew-proof sealant and preparation method thereof

    CN119463777A