Smashing-free brick with low water absorption rate and preparation method thereof

By using a combination of silane-modified polyether resin and other additives in tamper-free bricks, the existing tamper-free bricks have been solved, and high bonding strength, long life and good water resistance are achieved. ensures construction safety and material stability.

CN119019970APending Publication Date: 2024-11-26SHANGHAI NIUYUAN IND TRADE
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411083622.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing brick-free waterproof coating has poor bonding performance on the surface of ceramic tile, has a short service life, and contains free isocyanate that is harmful to the human body. It has construction safety risks and has a short time to resist water soaking, which is prone to secondary water leakage.

Method used

The water absorption rate is prepared by improving the polymerization process and curing conditions of the resin by improving the polymerization process and curing conditions of the resin. Low brick-free bricks ensure bonding strength and water resistance.

Benefits of technology

It achieves good bonding performance between the tiles and the surface of the ceramic tiles without smashing, extends the service life, improves water resistance and construction safety, shortens drying time, and avoids yellowing and cracking of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984522750000041
    Figure BDA0004984522750000041
  • Figure BDA0004984522750000051
    Figure BDA0004984522750000051
  • Figure BDA0004984522750000061
    Figure BDA0004984522750000061
Patent Text Reader

Abstract

The invention discloses a smashing-free brick with low water absorption rate. The smashing-free brick is prepared from the following raw materials in parts by weight: 90-99 parts of silane modified polyether resin, 1-5 parts of a silane coupling agent, 0.1-1 part of a light stabilizer, 0.5-1 part of a water removal agent and 0.01-1 part of a catalyst. The silane modified polyether resin is adopted, and the modification amount of silane in the silane modified polyether resin is 2.5%, so that the prepared smashing-free brick does not generate air holes, has better bonding performance with the surface of a ceramic tile, and is longer in service life. The combination of the epoxy silane coupling agent and the monoamino-modified silane coupling agent is adopted, so that the prepared smashing-free brick is good in appearance, high in bonding strength, short in surface drying time and simple and convenient to construct. The coating is good in environmental protection property, high in drying speed, capable of being put into use earlier, easy to construct through a single component, good in adhesive property and free of discoloration after deep curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a brick without smashing having low water absorption and a preparation method thereof, and relates to C09J, and in particular to the field of adhesives. Background Art

[0002] The kitchen and bathroom of a house are the places where the most water is used in family life. The kitchen and bathroom are the places where water leakage problems are most likely to occur. When water leakage occurs, the original tiles and waterproof layer need to be destroyed and waterproofed again, which is troublesome and costly to construct. The waterproof layer can be directly applied on the tiles by adopting the process of non-smashing bricks to achieve the effect of waterproofing and plugging leaks. The existing diurea non-smashing brick waterproof coating on the market has poor adhesion to the surface of tiles, is easy to peel off on the surface of tiles, and has a short service life. It also contains free isocyanates that are harmful to the human body, which is not conducive to construction safety. Therefore, it is very important to develop a non-smashing brick coating with good environmental performance and fast drying speed.

[0003] Chinese invention patent CN202211304136.2 discloses a brick-free interface material for repair and its preparation method. Silicone modification is added to the resin matrix and then combined with powder. The mechanical bite force between the inorganic adhesive and the exterior wall and the physical and chemical bonding force between the organic adhesive and the exterior wall can improve the service life of the exterior wall after repair or renovation, but it does not have a waterproof effect. Chinese invention patent CN202010446974.8 discloses a brick-free waterproof plugging composition based on alkoxysilicon-modified polymers. By preparing alkoxysilicon-modified polymers with a polyolefin main chain, brick-free waterproof plugging is performed, which is widely used in indoor kitchen and bathroom waterproof repairs. However, the water-resistant time is short, and there is a risk of secondary leakage in the later stage. Summary of the invention

[0004] In order to improve the water resistance of the non-smashing bricks and shorten the construction time, the first aspect of the present invention provides a non-smashing brick with low water absorption. The preparation raw materials include, by weight: 90-99 parts of silane-modified polyether resin, 1-5 parts of silane coupling agent, 0.1-1 parts of light stabilizer, 0.5-1 parts of dehydrating agent, and 0.01-1 parts of catalyst.

[0005] As a preferred embodiment, the mass proportion of silane modification in the silane-modified polyether resin is 1-5%.

[0006] As a preferred embodiment, the mass proportion of silane modification in the silane-modified polyether resin is 2-3%.

[0007] As a preferred embodiment, the mass proportion of the silane-modified resin in the silane-modified polyether resin is 2.5%.

[0008] During the experiment, the applicant found that the smash-free bricks prepared by using silane-modified polyether resin with a silane modification content of 2.5% would not produce pores, had poor adhesion to the ceramic tile surface, and had a longer service life. The possible reasons are speculated to be: in the silane-modified polyether resin, the modified silane content decreased and the polyether content increased, so that the methanol released during the curing process of the smash-free bricks can be smoothly discharged into the air, avoiding the methanol gas from remaining in the smash-free installation to form pores after the resin polymer is polymerized and sealed, thereby resulting in the problem of weak peeling resistance between the smash-free bricks and ceramic tiles and a short service life.

[0009] As a preferred embodiment, the silane coupling agent is selected from one or a combination of epoxy silane coupling agents, amino silane coupling agents, alkyl silane coupling agents, and aryl silane coupling agents.

[0010] As a preferred embodiment, the aminosilane coupling agent is a monoaminosilane coupling agent, and the monoaminosilane coupling agent is selected from one or a combination of 3-aminopropyltrimethoxysilane, Y-aminopropylmethyldiethoxysilane, and 3-aminopropyltriethoxysilane.

[0011] As a preferred embodiment, the aminosilane coupling agent is 3-aminopropyltrimethoxysilane.

[0012] As a preferred embodiment, the epoxy silane coupling agent is selected from one or a combination of γ-glycidyloxypropyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propyltriethoxysilane, 3-(2,3-epoxypropyloxy)propylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.

[0013] As a preferred embodiment, the epoxy silane coupling agent is γ-glycidyloxypropyltrimethoxysilane.

[0014] As a preferred embodiment, the silane coupling agent is a combination of an epoxy silane coupling agent and an amino silane coupling agent, and the weight ratio of the epoxy silane coupling agent to the amino silane coupling agent is 1:(0.2-2.5).

[0015] As a preferred embodiment, the weight ratio of the epoxy silane coupling agent to the amino silane coupling agent is 1:(1-2.5).

[0016] As a preferred embodiment, the weight ratio of the epoxy silane coupling agent to the amino silane coupling agent is 1:2.5.

[0017] The applicant found in the experiment that the combination of epoxy silane coupling agent and monoamino modified silane coupling agent as silane coupling agent can prepare a brick without smashing with good appearance and high bonding strength. The possible reason is that the combination of epoxy silane coupling agent and monoamino modified silane coupling agent promotes the polymerization of the chain segments in the silane modified polyether resin, provides an alkaline environment for the resin to play a catalytic role, improves the quality of deep curing, thereby achieving rapid polymerization and shortening the surface drying time. The applicant further found that the weight ratio of epoxy silane coupling agent and monoamino modified silane coupling agent is 1: (0.2-2.5), and the brick without smashing formed is not easy to crack and has a good appearance. The reason is that the silane coupling agent under the preferred weight ratio has high bonding strength. If it is not under the preferred weight ratio, the polymerization speed will be reduced, the surface drying time will be prolonged, and the internal polymerization effect of the brick without smashing formed is unstable and easy to crack.

[0018] As a preferred embodiment, the dewatering agent is vinyl alkoxysilane, and the vinyl alkoxysilane is selected from one or a combination of vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane, and vinyl triisopropoxysilane.

[0019] As a preferred embodiment, the dehydrating agent is vinyltrimethoxysilane.

[0020] During the experiment, the applicant found that the use of vinyltrimethoxysilane can remove water, improve the strength and hardness of the non-breakable bricks, and extend the service life of the non-breakable bricks. The possible reason is speculated to be: vinyltrimethoxysilane has a high reactivity and can react with the MS resin first to avoid the reaction of the resin with water vapor, thereby increasing the cross-linking degree of the resin, thereby improving the hardness and strength of the non-breakable bricks, facilitating production and extending the shelf life of the non-breakable bricks.

[0021] As a preferred embodiment, the light stabilizer is a liquid light stabilizer, and the viscosity of the light stabilizer at 20° C. is 1000-2000 mPa·s.

[0022] During the experiment, the applicant found that the introduction of a liquid light stabilizer with a viscosity of 1000-2000 mPa·s can increase the light resistance of the resin polymer, reduce the aging and decomposition reaction of the non-smashing coating on the surface of the tile, reduce the yellowing damage of the non-smashing bricks, and extend the service life of the material. In addition, the liquid light stabilizer with appropriate viscosity is evenly dispersed in the resin system and can react evenly, avoiding the problem of uneven dispersion of the solid stabilizer.

[0023] As a preferred embodiment, the catalyst is an organic tin catalyst, and the organic tin catalyst is selected from one or a combination of dibutyltin dilaurate, stannous octoate, and dibutyltin didodecylsulfide.

[0024] As a preferred embodiment, the catalyst is dibutyltin dilaurate.

[0025] In this application, dibutyltin dilaurate is used as a catalyst to increase the curing speed of the resin, adjust the surface drying time and the deep curing speed, shorten the construction time, and at the same time will not affect the appearance during the use of the non-smashing installation, and is not prone to cracking problems.

[0026] The second aspect of the present invention provides a method for preparing a brick without breaking with low water absorption, comprising the following steps:

[0027] S1: Mix and stir silane-modified polyether resin, epoxy silane coupling agent, light stabilizer and water scavenger at a stirring speed of 30-50 r / min and a dispersion time of 5-20 min;

[0028] S2 continues to add aminosilane coupling agent and catalyst, and disperses at high speed in vacuum, with a dispersion speed of 40-50r / min and a dispersion time of 10-20min;

[0029] After S3 stirring is completed, sampling is carried out and inspection is qualified.

[0030] As a preferred implementation, the vacuum pressure in step S2 is 0 to -0.1 MPa.

[0031] As a preferred implementation, the vacuum pressure in step S2 is -0.1 MPa.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The low water absorption bricks of the present invention are made of silane-modified polyether resin, wherein the modification amount of silane in the silane-modified polyether resin is 2.5%. The prepared bricks do not generate pores, have better bonding performance with the surface of ceramic tiles, and have a longer service life.

[0034] (2) The low water absorption bricks of the present invention are made of a combination of an epoxy silane coupling agent and a monoamino-modified silane coupling agent. The bricks have good appearance, high bonding strength, short surface drying time and are easy to construct.

[0035] (3) The low water absorption bricks of the present invention are made of epoxy silane coupling agent and monoamino-modified silane coupling agent in a weight ratio of 1: (0.2-2.5), which can reduce the water absorption of the bricks, achieve good appearance, and have excellent water whitening resistance.

[0036] (4) The low water absorption bricks of the present invention can improve the strength and hardness of the bricks and extend their service life by introducing vinyl trimethoxy silane as a dehydrating agent.

[0037] (5) The bricks without smashing due to low water absorption of the present invention are environmentally friendly, dry quickly, can be put into use earlier, are easy to construct with a single component, have good bonding properties, and do not change color after deep curing. DETAILED DESCRIPTION

[0038] Example

[0039] A brick with low water absorption and free from smashing, the raw materials for preparation are calculated by weight: see Table 1 below for details:

[0040] Table 1

[0041]

[0042]

[0043] The silane-modified polyether resin has a mass proportion of 2.5% and is purchased from Prudentia with a brand number of HP213.

[0044] The light stabilizer is a liquid light stabilizer with a viscosity of 1000-2000 mPa·s at 20° C. It is purchased from Canghong Industry with a brand number of 1830.

[0045] The epoxy silane coupling agent is γ-glycidyloxypropyl trimethoxysilane, purchased from Sibao, brand GX-560. The aminosilane coupling agent of Examples 1-4 and Comparative Example 2 is 3-aminopropyl trimethoxysilane, purchased from Sibao, brand GX-540; the aminosilane coupling agent of Comparative Example 1 is oligomeric bisaminosilane, purchased from Sibao, brand GX-1146.

[0046] The vinyl trimethoxysilane was purchased from Sibao with the brand name GX-171.

[0047] The dibutyltin dilaurate was purchased from Mannheimer Schmidt Chemicals with the brand name TMG128.

[0048] A method for preparing a brick without breaking with low water absorption comprises the following steps:

[0049] S1: Mix and stir silane-modified polyether resin, epoxy silane coupling agent, light stabilizer and water scavenger at a stirring speed of 40 r / min and a dispersion time of 10 min;

[0050] S2 continues to add aminosilane coupling agent and catalyst, and disperses at high speed in vacuum, with a dispersion speed of 45r / min and a dispersion time of 20min;

[0051] After S3 stirring is completed, sampling is carried out and inspection is qualified.

[0052] The vacuum pressure in step S2 is -0.1 MPa.

[0053] Comparative Example 3

[0054] A brick that does not require breaking, purchased from Wacker.

[0055] Comparative Example 4

[0056] A brick that doesn't need to be smashed, purchased from Waterpool.

[0057] Performance Testing

[0058] 1. Base surface cleaning:

[0059] 1.1.1 Clean the stains on the tile surface and the edges of the gaps to ensure that the surface of the caulking material is solid;

[0060] 1.1.2 Clean up the sealant residue;

[0061] 1.1.3 Wider cracks should be repaired in advance.

[0062] 2. Construction method

[0063] 2.1 Seal the floor drain area to prevent materials from flowing into the floor drain;

[0064] 2.2 Pour the bricks to be applied in the area to be constructed, and use a plastic serrated scraper to level them. Pay attention to defoaming and uniformity of coating. You can also use a brush to assist in coating.

[0065] Note: Apply slowly and evenly during construction to reduce the generation of bubbles. If there are many bubbles, use a hot air gun to blow them away before the product dries.

[0066] 3. Construction and maintenance

[0067] The material needs to be cured for 24 hours after construction before it can be used normally.

[0068] The performance of non-smashing bricks was tested with reference to the Q / NYMS 01-2024 standard. The test standard for 24h deep curing speed was based on the GB / T32369-2015 wedge groove method. The test results are shown in Table 2 below.

[0069] Table 2

[0070]

[0071]

Claims

1. A brick with low water absorption and free from smashing, characterized in that: The raw materials for preparation include, by weight: 90-99 parts of silane-modified polyether resin, 1-5 parts of silane coupling agent, 0.1-1 parts of light stabilizer, 0.5-1 parts of water remover and 0.01-1 parts of catalyst.

2. The low water absorption brick according to claim 1, characterized in that: The mass proportion of the silane-modified resin in the silane-modified polyether resin is 1-5%.

3. The low water absorption brick according to claim 1, characterized in that: The silane coupling agent is selected from one or a combination of epoxy silane coupling agents, amino silane coupling agents, alkyl silane coupling agents, and aryl silane coupling agents.

4. The low water absorption brick according to claim 3, characterized in that: The aminosilane coupling agent is a monoaminosilane coupling agent, and the monoaminosilane coupling agent is selected from one or a combination of 3-aminopropyltrimethoxysilane, Y-aminopropylmethyldiethoxysilane, and 3-aminopropyltriethoxysilane.

5. The low water absorption brick according to claim 3, characterized in that: The epoxy silane coupling agent is selected from one or a combination of γ-glycidyloxypropyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propyltriethoxysilane, 3-(2,3-epoxypropyloxy)propylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.

6. The low water absorption brick according to claim 1, characterized in that: The silane coupling agent is a combination of an epoxy silane coupling agent and an amino silane coupling agent, and the weight ratio of the epoxy silane coupling agent to the amino silane coupling agent is 1:(0.2-2.5).

7. The low water absorption brick according to claim 1, characterized in that: The dewatering agent is vinyl alkoxysilane, and the vinyl alkoxysilane is selected from one or a combination of vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane, and vinyl triisopropoxysilane.

8. The low water absorption brick according to claim 1, characterized in that: The light stabilizer is a liquid light stabilizer, and the viscosity of the light stabilizer at 20° C. is 1000-2000 mPa·s.

9. The low water absorption brick according to claim 1, characterized in that: The catalyst is an organic tin catalyst, and the organic tin catalyst is selected from one or a combination of dibutyltin dilaurate, stannous octoate, and dibutyltin didodecylsulfide.

10. A method for preparing a brick with low water absorption and free from smashing according to any one of claims 3 to 9, characterized in that: The following steps are involved: S1: Mix and stir silane-modified polyether resin, epoxy silane coupling agent, light stabilizer and water scavenger at a stirring speed of 30-50 r / min and a dispersion time of 5-20 min; S2 continues to add aminosilane coupling agent and catalyst, and disperses at high speed in vacuum, with a dispersion speed of 40-50r / min and a dispersion time of 10-20min; After S3 stirring is completed, sampling is carried out and inspection is qualified.

Citation Information

Patent Citations

  • Brick-smashing-free leaking stoppage waterproof composition based on alkoxy silicon modified polymer

    CN111607358A

  • Brick-smashing-free interface material for repairing and preparation method of brick-smashing-free interface material

    CN115584152A