By combining microjet technology and low-temperature spray drying, microcapsule phase change material particles with particle size less than 200 nanometers and uniform particle size are formed, which solves the problem of difficult particle size to reach 200 nanometers and poor dispersion in traditional technology, and improves the problem of Control accuracy of core content and particle size.
Patent Information
- Application Number
- CN202310591013.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
The particles of traditional microcapsule phase change material are difficult to reach a particle size below 200 nanometers, and have a large dispersion of the particle size and a large wall thickness, resulting in a low core content and difficult to accurately control.
Emulsions using n-octadecane, polyurethane monomer, isocyanate, surfactant, polyvinyl alcohol, polyethylene glycol, chain extender and other components form nano-scale particles through microjets, and are instantly carried out under the action of MOFs-supported high-efficiency catalyst. The interfacial polymerization reaction of states forms microcapsules, and microcapsule phase change material particles with particle size less than 200 nanometers and uniform particle size are obtained by low-temperature spray drying.
The particle size of the microcapsule phase change material particles is less than 200 nanometers, and the particle size is relatively uniform. The core content of the microcapsule reaches 80%, solving the problem that the particle size is difficult to accurately control.
Smart Images

Figure CN119019987A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and particularly relates to nanometer-scale microcapsule phase change material particles and a preparation method thereof. Background Art
[0002] Microcapsule phase change materials are tiny particles with phase change properties made by microencapsulating phase change materials. They can absorb or release heat when the temperature or pressure changes. At present, microcapsule phase change materials have been widely used in the fields of construction, thermal management, textiles, and medical treatment. Particle size and core material content are two important parameters of microcapsule phase change materials, which determine the performance and application range of the material.
[0003] Traditional microcapsule phase change materials control the size of microcapsule phase change material particles by stirring and controlling the flow rate of the emulsion. However, the particle size of the microcapsule phase change material particles produced by this control method is difficult to reach below 200 nanometers, and the particle size dispersion is large and the wall thickness is large. Summary of the invention
[0004] In view of the above problems, the present invention provides a nanometer-scale microcapsule phase change material particle and a preparation method thereof. The particle size of the microcapsule phase change material particle is less than 200 nanometers and the particle size is relatively uniform, and the core material content of the microcapsule reaches 80%.
[0005] A nanometer-scale microcapsule phase change material particle, the raw materials and components of the microcapsule phase change material particle include: 70-130 parts of n-octadecane, 30-50 parts of polyurethane monomer, 40-70 parts of isocyanate, 22-44 parts of surfactant, 14-25 parts of polyvinyl alcohol, 48-112 parts of polyethylene glycol, 13-36 parts of chain extender, 3-6 parts of high-efficiency catalyst and 1100-1800 parts of water.
[0006] Furthermore, the surfactant is one or more of silicone surfactant, sodium dodecylbenzene sulfonate, nonylphenol polyethylene glycol, random polystyrene-maleic anhydride, polyethylene glycol octylphenyl ether, polyvinyl alcohol, Tween-20, Tween-80, and Span-20.
[0007] Furthermore, the chain extender is one or more of ethylene glycol, 1,4-butanediol, 1,6-hexanediol, glycerol, trimethylolpropane, and triethylolpropane.
[0008] Furthermore, the high-efficiency catalyst is one of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl), triethanolamine, triethylenediamine, stannous octoate, and zinc octoate.
[0009] On the other hand, the present invention provides a method for preparing nano-scale microcapsule phase change material particles, comprising:
[0010] Evenly mixing n-octadecane, polyurethane monomer, isocyanate, surfactant, polyvinyl alcohol, polyethylene glycol and chain extender to obtain a mixture;
[0011] Slowly adding the mixture into water while stirring to obtain a dispersed emulsion;
[0012] The emulsion is placed in a preparation device, and the emulsion is input into a disperser by controlling a supercharger to obtain phase change material particles;
[0013] The phase change material particles are input into an interfacial polymerization pipeline, and under the action of the efficient catalyst supported by MOFs, the shell material monomers complete a transient polymerization reaction on the surface of the phase change material particles, so that the phase change material particles are microencapsulated to obtain microcapsule particles;
[0014] Drying the microcapsule particles by low-temperature spraying, and separating the microcapsules from the catalyst according to different densities to obtain microcapsule powder;
[0015] The microcapsule powder is dried to obtain microcapsule phase change material particles.
[0016] Furthermore, the step of inputting the emulsion into the disperser by controlling the supercharger to obtain the phase change material particles includes: adjusting the size of the phase change material particles by controlling the pressure of the supercharger.
[0017] Furthermore, the disperser is circulated and cooled by water cooling.
[0018] Furthermore, the preparation equipment comprises:
[0019] A liquid storage barrel, a liquid outlet pipe with a one-way valve is installed at the bottom of the liquid storage barrel;
[0020] A supercharger, wherein the inlet of the supercharger is connected to one end of the liquid outlet pipe;
[0021] A disperser, wherein the inlet of the disperser is connected to the outlet of the supercharger through a pipeline;
[0022] an interfacial polymerization pipeline, wherein the inlet of the interfacial polymerization pipeline is connected to the outlet of the disperser;
[0023] A low-temperature atomization device, wherein the inlet of the low-temperature atomization device is connected to the outlet of the interfacial polymerization pipeline.
[0024] Furthermore, a water cooling pipe is provided in the disperser.
[0025] Furthermore, a pressure gauge is installed on the pipeline.
[0026] The beneficial effects of the present invention are as follows: the present invention adds n-octadecane, polyurethane monomer, isocyanate, surfactant, polyvinyl alcohol, polyethylene glycol and chain extender into water to obtain a dispersed emulsion, forms nano-scale homogeneous particles through micro-jetting, and carries out an interfacial polymerization reaction in a pipeline through MOFs loaded with a high-efficiency catalyst to form microcapsules, and then obtains microcapsule powder through low-temperature spray drying, thereby solving the problem that microcapsule phase change material particles cannot be homogeneously dispersed in liquid and precipitate is generated, so that the particle size of the microcapsule phase change material particles is less than 200 nanometers and the particle size is relatively uniform, and the core material content of the microcapsule reaches 80%, thereby solving the problem that the particle size of the microcapsule phase change material is difficult to reach below 200 nanometers, the core material content is low due to the large thickness of the phase change wall material, and the particle size cannot be more accurately controlled. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 A schematic diagram of the structure of a preparation device in an embodiment of the present invention is shown;
[0029] Figure 2 The flowchart of a method for preparing nano-scale microcapsule phase change material particles in an embodiment of the present invention is shown.
[0030] In the figure: 1. Liquid storage barrel; 2. One-way valve; 3. Liquid outlet pipe; 4. Supercharger; 5. Disperser; 6. Pipeline; 7. Interfacial polymerization pipeline; 8. Low-temperature atomization device; 9. Pressure gauge. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The embodiment of the present invention provides a nanometer-scale microcapsule phase change material particle, and the particle material is composed of a phase change material (core material) and an emulsion.
[0033] Among them, the phase change material (core material) is selected from n-octadecane, aliphatic hydrocarbons, paraffin, fatty acids, fatty acid esters, etc.; the emulsion is prepared by adding the core material, shell material, emulsifier, surfactant, chain extender, etc. into water and mixing them.
[0034] Furthermore, the components of the shell material may be polymethyl acrylate monomer, polyurethane monomer, etc.; emulsifier: one or more of sodium dodecylbenzene sulfonate, Tween-60, Tween-80, and polyvinyl alcohol.
[0035] Specifically, when preparing nano-scale microcapsule phase change material particles, a preparation device is used to form nano-scale isotropic particles through micro-jet, and an efficient catalyst is used in a pipeline to instantaneously complete an interfacial polymerization reaction to form microcapsules, which are then spray-dried at low temperature to obtain microcapsule powder.
[0036] like Figure 1 As shown, the preparation equipment includes: a liquid storage tank 1, a supercharger 4, a disperser 5, an interfacial polymerization pipeline 7, and a low-temperature atomization device 8.
[0037] The bottom of the liquid storage barrel 1 is provided with a liquid outlet pipe 3 with a one-way valve 2; the inlet of the supercharger 4 is connected to one end of the liquid outlet pipe 3; the inlet of the disperser 5 is connected to the outlet of the supercharger 4 through a pipe 6; the inlet of the interfacial polymerization pipe 7 is connected to the outlet of the disperser 5; the inlet of the low-temperature atomization device 8 is connected to the outlet of the interfacial polymerization pipe 7. Specifically, a water cooling pipe is provided in the disperser 5, and a pressure gauge 9 is installed on the pipe 6.
[0038] The following is an explanation using n-octadecane micro-core material and polyurethane monomer shell material as examples.
[0039] Example 1
[0040] Exemplarily, the raw materials and components of the microcapsule phase change material particles include: 70 parts of n-octadecane, 30 parts of polyurethane monomer, 40 parts of isocyanate, 22 parts of surfactant, 14 parts of polyvinyl alcohol, 48 parts of polyethylene glycol, 13 parts of chain extender, 3 parts of high-efficiency catalyst, and 1100 parts of water.
[0041] Specifically, the surfactant is one or more of silicone surfactant, sodium dodecylbenzene sulfonate, nonylphenol polyethylene glycol, random polystyrene-maleic anhydride, polyethylene glycol octylphenyl ether, polyvinyl alcohol, Tween-20, Tween-80, and Span-20.
[0042] Specifically, the chain extender is one or more of ethylene glycol, 1,4-butanediol, 1,6-hexanediol, glycerol, trimethylolpropane, and triethylolpropane.
[0043] Specifically, the high-efficiency catalyst is one of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl), triethanolamine, triethylenediamine, stannous octoate, and zinc octoate.
[0044] like Figure 2 As shown, when preparing nano-scale microcapsule phase change material particles, the following steps are included:
[0045] 70 parts of n-octadecane, 30 parts of polyurethane monomer, 40 parts of isocyanate, 22 parts of surfactant, 14 parts of polyvinyl alcohol, 48 parts of polyethylene glycol and 13 parts of chain extender were mixed uniformly to obtain a mixture;
[0046] Slowly add the mixture into 1100 parts of water while stirring to obtain a dispersed emulsion;
[0047] The emulsion is placed in the preparation equipment, and the emulsion is input into the disperser by controlling the supercharger to obtain phase change material particles; in addition, the size of the phase change material particles is adjusted by controlling the pressure of the supercharger. For example, 11-12MPa can obtain material particles with a particle size of about 200 nanometers. In addition, the greater the pressure, the greater the impact of the phase change material in the disperser, so the larger phase change material will become nanometer-level. For specific particle size control, the corresponding pressure should be controlled according to the type of phase change material. Taking n-octadecane core material and polyurethane shell material as an example, when the pressure is controlled at 7.9MPa, microcapsules with a particle size of 800 nanometers are produced, and when the pressure is controlled at 11.8MPa, microcapsules with a particle size of 200 nanometers are produced. When the pressure is adjusted to 13.6Mpa and above, microcapsules with a particle size of 110 nanometers can be produced. When the pressure is adjusted to about 14MPa or above, microcapsules with a particle size less than 110 nanometers but uneven particle size can be produced. To produce microcapsules between 110 and 800 nanometers, the corresponding control pressure is obtained by using quadratic function interpolation based on the above data range.
[0048] Furthermore, the disperser is cooled while dispersing, and conventional water cooling (20 degrees Celsius) is used for cooling. The main function is that the emulsion collides in the disperser (dispersing unit), which will increase the temperature in the dispersion unit. If the temperature is too high, the shell material may react without a catalyst. Therefore, water at a temperature of 20 degrees Celsius or below is used to circulate and cool the dispersion unit. The disperser uses micro-jet technology, and its structure can be in various forms. Its main function is to allow the emulsion to be fully mixed and collided in the disperser under pressure to produce a phase change material with a smaller particle size.
[0049] The phase change material particles are input into the interfacial polymerization pipeline. Under the action of 3 parts of the high-efficiency catalyst supported by MOFs, the shell material monomer completes a transient polymerization reaction on the surface of the phase change material particles, so that the phase change material particles are microencapsulated to obtain microcapsule particles. Specifically, the high-efficiency catalyst is selected according to the type of shell material. For example, if polyurethane is used, the catalyst can be one of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl), triethanolamine, triethylenediamine, stannous octoate, and zinc octoate.
[0050] The microcapsule particles are dried by low-temperature spraying, and the microcapsules are separated from the catalyst according to the difference in density to obtain microcapsule powder; specifically, the atomizing device uses a conventional scattering nozzle (the principle is similar to that of an air humidifier) to form a spray of the emulsion after the reaction. There is not much water in the emulsion, and the water in the emulsion can be evaporated at room temperature after forming a spray, thereby achieving the purpose of drying. The density does not need to be judged, but the different densities of the microcapsules are used to spray out at different distances, so that the catalyst and the microcapsules can be separated and a part of the catalyst can be recovered.
[0051] The microcapsule powder is dried to obtain microcapsule phase change material particles; specifically, drying here means separating the microcapsules in the emulsion, rather than suspending them in water. The temperature is room temperature, but the humidity of the air should not be too high, generally the relative humidity is less than 80%.
[0052] Example 2
[0053] Exemplarily, the raw materials and components of the microcapsule phase change material particles include: 105 parts of n-octadecane, 40 parts of polyurethane monomer, 60 parts of isocyanate, 33 parts of surfactant, 20 parts of polyvinyl alcohol, 80 parts of polyethylene glycol, 25 parts of chain extender, 4 parts of high-efficiency catalyst, and 1400 parts of water.
[0054] Specifically, the surfactant is one or more of silicone surfactant, sodium dodecylbenzene sulfonate, nonylphenol polyethylene glycol, random polystyrene-maleic anhydride, polyethylene glycol octylphenyl ether, polyvinyl alcohol, Tween-20, Tween-80, and Span-20.
[0055] Specifically, the chain extender is one or more of ethylene glycol, 1,4-butanediol, 1,6-hexanediol, glycerol, trimethylolpropane, and triethylolpropane.
[0056] Specifically, the high-efficiency catalyst is one of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl), triethanolamine, triethylenediamine, stannous octoate, and zinc octoate.
[0057] like Figure 2As shown, when preparing nano-scale microcapsule phase change material particles, the following steps are included:
[0058] 105 parts of n-octadecane, 40 parts of polyurethane monomer, 60 parts of isocyanate, 33 parts of surfactant, 20 parts of polyvinyl alcohol, 80 parts of polyethylene glycol, and 25 parts of chain extender were uniformly mixed to obtain a mixture;
[0059] Slowly add the mixture into 1400 parts of water while stirring to obtain a dispersed emulsion;
[0060] The emulsion is placed in the preparation equipment, and the emulsion is input into the disperser by controlling the supercharger to obtain phase change material particles; in addition, the size of the phase change material particles is adjusted by controlling the pressure of the supercharger. For example, 11-12MPa can obtain material particles with a particle size of about 200 nanometers. In addition, the greater the pressure, the greater the impact of the phase change material in the disperser, so the larger phase change material will become nanometer-level. For specific particle size control, the corresponding pressure should be controlled according to the type of phase change material. Taking n-octadecane core material and polyurethane shell material as an example, when the pressure is controlled at 7.9MPa, microcapsules with a particle size of 800 nanometers are produced, and when the pressure is controlled at 11.8MPa, microcapsules with a particle size of 200 nanometers are produced. When the pressure is adjusted to 13.6Mpa and above, microcapsules with a particle size of 110 nanometers can be produced. When the pressure is adjusted to about 14MPa or above, microcapsules with a particle size less than 110 nanometers but uneven particle size can be produced. To produce microcapsules between 110 and 800 nanometers, the corresponding control pressure is obtained by using quadratic function interpolation based on the above data range.
[0061] Furthermore, the disperser is cooled while dispersing, and conventional water cooling (20 degrees Celsius) is used for cooling. The main function is that the emulsion collides in the disperser (dispersing unit), which will increase the temperature in the dispersion unit. If the temperature is too high, the shell material may react without a catalyst. Therefore, water at a temperature of 20 degrees Celsius or below is used to circulate and cool the dispersion unit. The disperser uses micro-jet technology, and its structure can be in various forms. Its main function is to allow the emulsion to be fully mixed and collided in the disperser under pressure to produce a phase change material with a smaller particle size.
[0062] The phase change material particles are input into an interfacial polymerization pipeline. Under the action of 4 parts of a high-efficiency catalyst loaded on MOFs, a transient polymerization reaction occurs on the surface of the shell material monomer phase change material particles, so that the phase change material particles are microencapsulated to obtain microcapsule particles. Specifically, different high-efficiency catalysts are selected according to the type of shell material. For example, if polyurethane is used, the catalyst can be one of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl), triethanolamine, triethylenediamine, stannous octoate, and zinc octoate.
[0063] The microcapsule particles are dried by low-temperature spraying, and the microcapsules are separated from the catalyst according to the difference in density to obtain microcapsule powder; specifically, the atomizing device uses a conventional scattering nozzle (the principle is similar to that of an air humidifier) to form a spray of the emulsion after the reaction. There is not much water in the emulsion, and the water in the emulsion can be evaporated at room temperature after forming a spray, thereby achieving the purpose of drying. The density does not need to be judged, but the different densities of the microcapsules are used to spray out at different distances, so that the catalyst and the microcapsules can be separated and a part of the catalyst can be recovered.
[0064] The microcapsule powder is dried to obtain microcapsule phase change material particles; specifically, drying here means separating the microcapsules in the emulsion, rather than suspending them in water. The temperature is room temperature, but the humidity of the air should not be too high, generally the relative humidity is less than 80%.
[0065] Example 3
[0066] Exemplarily, the raw materials and components of the microcapsule phase change material particles include: 130 parts of n-octadecane, 50 parts of polyurethane monomer, 70 parts of isocyanate, 44 parts of surfactant, 25 parts of polyvinyl alcohol, 112 parts of polyethylene glycol, 36 parts of chain extender, 6 parts of high-efficiency catalyst, and 1800 parts of water.
[0067] Specifically, the surfactant is one or more of silicone surfactant, sodium dodecylbenzene sulfonate, nonylphenol polyethylene glycol, random polystyrene-maleic anhydride, polyethylene glycol octylphenyl ether, polyvinyl alcohol, Tween-20, Tween-80, and Span-20.
[0068] Specifically, the chain extender is one or more of ethylene glycol, 1,4-butanediol, 1,6-hexanediol, glycerol, trimethylolpropane, and triethylolpropane.
[0069] Specifically, the high-efficiency catalyst is one of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl), triethanolamine, triethylenediamine, stannous octoate, and zinc octoate.
[0070] like Figure 2As shown, when preparing nano-scale microcapsule phase change material particles, the following steps are included:
[0071] 130 parts of n-octadecane, 50 parts of polyurethane monomer, 70 parts of isocyanate, 44 parts of surfactant, 25 parts of polyvinyl alcohol, 112 parts of polyethylene glycol, and 36 parts of chain extender were mixed uniformly to obtain a mixture;
[0072] Slowly add the mixture into 1800 parts of water while stirring to obtain a dispersed emulsion;
[0073] The emulsion is placed in the preparation equipment, and the emulsion is input into the disperser by controlling the supercharger to obtain phase change material particles; in addition, the size of the phase change material particles is adjusted by controlling the pressure of the supercharger. For example, 11-12MPa can obtain material particles with a particle size of about 200 nanometers. In addition, the greater the pressure, the greater the impact of the phase change material in the disperser, so the larger phase change material will become nanometer-level. For specific particle size control, the corresponding pressure should be controlled according to the type of phase change material. Taking n-octadecane core material and polyurethane shell material as an example, when the pressure is controlled at 7.9MPa, microcapsules with a particle size of 800 nanometers are produced, and when the pressure is controlled at 11.8MPa, microcapsules with a particle size of 200 nanometers are produced. When the pressure is adjusted to 13.6Mpa and above, microcapsules with a particle size of 110 nanometers can be produced. When the pressure is adjusted to about 14MPa or above, microcapsules with a particle size less than 110 nanometers but uneven particle size can be produced. To produce microcapsules between 110 and 800 nanometers, the corresponding control pressure is obtained by using quadratic function interpolation based on the above data range.
[0074] Furthermore, the disperser is cooled while dispersing, and conventional water cooling (20 degrees Celsius) is used for cooling. The main function is that the emulsion collides in the disperser (dispersing unit), which will increase the temperature in the dispersion unit. If the temperature is too high, the shell material monomer may react without a catalyst. Therefore, water at a temperature of 20 degrees Celsius or below is used to circulate and cool the dispersion unit. The disperser uses micro-jet technology, and its structure can be in various forms. Its main function is to allow the emulsion to be fully mixed and collided in the disperser under pressure to produce a phase change material with a smaller particle size.
[0075] The phase change material particles are input into the interfacial polymerization pipeline. Under the action of 6 parts of the high-efficiency catalyst loaded by MOFs, the shell material monomer completes a transient polymerization reaction on the surface of the phase change material particles, so that the phase change material particles are microencapsulated to obtain microcapsule particles. Specifically, the high-efficiency catalyst is selected according to the type of shell material. For example, if polyurethane is used, the catalyst can be one of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl), triethanolamine, triethylenediamine, stannous octoate, and zinc octoate.
[0076] The microcapsule particles are dried by low-temperature spraying, and the microcapsules are separated from the catalyst according to the difference in density to obtain microcapsule powder; specifically, the atomizing device uses a conventional scattering nozzle (the principle is similar to that of an air humidifier) to form a spray of the emulsion after the reaction. There is not much water in the emulsion, and the water in the emulsion can be evaporated at room temperature after forming a spray, thereby achieving the purpose of drying. The density does not need to be judged, but the different densities of the microcapsules are used to spray out at different distances, so that the catalyst and the microcapsules can be separated and a part of the catalyst can be recovered.
[0077] The microcapsule powder is dried to obtain microcapsule phase change material particles; specifically, drying here means separating the microcapsules in the emulsion, rather than suspending them in water. The temperature is room temperature, but the humidity of the air should not be too high, generally the relative humidity is less than 80%.
[0078] When implementing Examples 1-3, the ingredients of the raw materials are as follows:
[0079]
[0080]
[0081] The invention adds n-octadecane, polyurethane monomer, isocyanate, surfactant, polyvinyl alcohol, polyethylene glycol and chain extender into water to obtain dispersed emulsion, forms nanometer-scale homogeneous particles through micro-jet, instantaneously completes interfacial polymerization reaction through high-efficiency catalyst in a pipeline to form microcapsules, and then obtains microcapsule powder through low-temperature spray drying, thereby solving the problem that microcapsule phase change material particles cannot be homogeneously dispersed in liquid and precipitate is generated, so that the particle size of microcapsule phase change material particles is less than 200 nanometers and the particle size is relatively uniform, and the core material content of the microcapsule reaches 80%, thereby solving the problem that the particle size of microcapsule phase change material is difficult to reach below 200 nanometers, the core material content is low due to the large thickness of phase change wall material, and the particle size cannot be accurately controlled.
[0082] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A nanometer-scale microcapsule phase change material particle, characterized in that: The raw materials and components of the microcapsule phase change material particles include: 70-130 parts of n-octadecane, 30-50 parts of polyurethane monomer, 40-70 parts of isocyanate, 22-44 parts of surfactant, 14-25 parts of polyvinyl alcohol, 48-112 parts of polyethylene glycol, 13-36 parts of chain extender, 3-6 parts of high-efficiency catalyst and 1100-1800 parts of water.
2. The nanometer-scale microcapsule phase change material particle according to claim 1, characterized in that: The surfactant is one or more of an organosilicon surfactant, sodium dodecylbenzene sulfonate, nonylphenol polyethylene glycol, random polystyrene-maleic anhydride, polyethylene glycol octylphenyl ether, polyvinyl alcohol, Tween-20, Tween-80, and Span-20.
3. The nanometer-scale microcapsule phase change material particle according to claim 1, characterized in that: The chain extender is one or more of ethylene glycol, 1,4-butanediol, 1,6-hexanediol, glycerol, trimethylolpropane, and triethylolpropane.
4. The nano-scale microcapsule phase change material particle according to claim 1, characterized in that: The high-efficiency catalyst is one of N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl), triethanolamine, triethylenediamine, stannous octoate and zinc octoate.
5. A method for preparing nano-scale microcapsule phase change material particles according to claim 1, characterized in that: include: Evenly mixing n-octadecane, polyurethane monomer, isocyanate, surfactant, polyvinyl alcohol, polyethylene glycol and chain extender to obtain a mixture; Slowly adding the mixture into water while stirring to obtain a dispersed emulsion; The emulsion is placed in a preparation device, and the emulsion is input into a disperser by controlling a supercharger to obtain phase change material particles; The phase change material particles are input into an interfacial polymerization pipeline, and under the action of the efficient catalyst supported by MOFs, the shell material monomers complete a transient polymerization reaction on the surface of the phase change material particles, so that the phase change material particles are microencapsulated to obtain microcapsule particles; Drying the microcapsule particles by low-temperature spraying, and separating the microcapsules from the catalyst according to different densities to obtain microcapsule powder; The microcapsule powder is dried to obtain microcapsule phase change material particles.
6. The method for preparing nano-scale microcapsule phase change material particles according to claim 5, characterized in that: The method of inputting the emulsion into the disperser by controlling the supercharger to obtain the phase change material particles includes: adjusting the size of the phase change material particles by controlling the pressure of the supercharger.
7. The method for preparing nano-scale microcapsule phase change material particles according to claim 6, characterized in that: The disperser is circulated and cooled by water cooling.
8. The method for preparing nano-scale microcapsule phase change material particles according to claim 5, characterized in that: The preparation equipment comprises: A liquid storage barrel, a liquid outlet pipe with a one-way valve is installed at the bottom of the liquid storage barrel; A supercharger, wherein the inlet of the supercharger is connected to one end of the liquid outlet pipe; A disperser, wherein the inlet of the disperser is connected to the outlet of the supercharger through a pipeline; an interfacial polymerization pipeline, wherein the inlet of the interfacial polymerization pipeline is connected to the outlet of the disperser; A low-temperature atomization device, wherein the inlet of the low-temperature atomization device is connected to the outlet of the interfacial polymerization pipeline.
9. The method for preparing nano-scale microcapsule phase change material particles according to claim 8, characterized in that: A high-efficiency catalyst supported by MOFs is placed in the interfacial polymerization pipeline.