Heat-conducting wave-absorbing material and preparation method thereof
Magnetic carbon oxide nanotubes are prepared by using co-precipitation reaction in thermally absorbing materials, and arranged in a directional manner in the magnetic field, combining vinyl silicone oil and hydrogen-containing silicone oil, the contradiction between thermal conductivity and wave absorption performance is solved, and thermal conductivity and The synchronous improvement of wave absorbing performance maintains mechanical performance and is suitable for sensitive electronic devices.
Patent Information
- Application Number
- CN202411055736.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-26
AI Technical Summary
There are contradictions in the improvement of thermal conductivity and wave absorption properties of existing thermal conductivity and wave absorption properties, and it is difficult to take into account both. High filling leads to a decrease in mechanical properties, which cannot meet the requirements of sensitive electronic devices for both electromagnetic wave absorption and efficient thermal conduction capabilities.
By co-precipitation reaction of trivalent iron salt, divalent iron salt and carbon oxide nanotubes, magnetic carbon oxide nanotubes are prepared and arranged in a directional manner in the magnetic field, combining vinyl silicone oil and hydrogen-containing silicone oil to prepare heat conduction A wave-absorbing material uses the magnetic and thermal conductivity of iron tetroxide to achieve synchronous improvement of the material's thermal conductivity and wave-absorbing performance.
At a lower filling ratio, the thermal conductivity of the material is significantly improved, and it has both thermal conductivity and wave absorption properties, avoids the mutual suppression of thermal conductivity and wave absorption properties, and maintains the mechanical properties of the material. It is suitable for sensitive electronic devices.
Smart Images

Figure CN119019996A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of heat-conducting and wave-absorbing materials, and in particular to a heat-conducting and wave-absorbing material and a preparation method thereof. Background Art
[0002] In recent years, the size of electronic devices represented by semiconductor components has become smaller and smaller, and the heat generation has continued to increase. At the same time, the electromagnetic interference problem that comes with it has become more and more serious. The use of thermal conductive wave absorbing materials can effectively reduce the operating temperature of electronic components, while reducing or shielding the electromagnetic clutter they generate. The overall research and development ideas of thermal conductive wave absorbing materials are roughly the same, that is, adding functional fillers to the polymer matrix to make the material have thermal conductivity or wave absorbing functions. Generally, by mixing and adding traditional thermal conductive fillers and wave absorbing agents into the matrix material, a material with both thermal conductive and wave absorbing functions is obtained. However, since there is an upper limit to the total amount of functional fillers added in matrix materials such as rubber, the increase in the amount of a certain (thermal conductive, wave absorbing) filler will inevitably lead to a decrease in the amount of another functional filler added, resulting in a contradiction between the thermal conductivity and wave absorbing properties of thermal conductive wave absorbing materials, making it difficult to achieve the simultaneous improvement of the thermal conductivity and wave absorbing properties of the material. At present, the research and development of thermal conductive wave absorbing materials can only balance the thermal conductivity and wave absorbing performance indicators of the material by comprehensively coordinating the addition ratio of the two fillers, which cannot meet the requirements of sensitive electronic devices for materials with both electromagnetic wave absorption function and efficient heat conduction ability.
[0003] In addition, traditional dual-functional filler thermally conductive and wave-absorbing composite materials require high filling of thermal conductors and absorbers at the same time, which will lead to a significant decrease in the mechanical properties of the composite materials. Summary of the invention
[0004] The main purpose of the present invention is to provide a heat-conducting and wave-absorbing material and a preparation method thereof, aiming to solve the problems of existing heat-conducting and wave-absorbing materials that the thermal conductivity and wave-absorbing properties cannot be taken into account at the same time and the mechanical properties are poor.
[0005] To achieve the above object, the present invention provides a method for preparing a thermal conductive wave absorbing material, comprising the following steps:
[0006] S10, mixing a trivalent iron salt, a divalent iron salt, a precipitant, water and oxidized carbon nanotubes to perform a coprecipitation reaction to obtain magnetic oxidized carbon nanotubes;
[0007] S20, mixing magnetic oxidized carbon nanotubes, vinyl silicone oil, and hydrogen-containing silicone oil to obtain a mixture, placing the mixture in a magnetic field to orient the magnetic oxidized carbon nanotubes along the direction of the magnetic field, and thermally curing the mixture after the orientation is completed to obtain a thermal conductive wave absorbing material;
[0008] Wherein, the mass ratio of the magnetic oxidized carbon nanotubes, vinyl silicone oil and hydrogen-containing silicone oil is (10-30): (50-100): (0.4-1.5).
[0009] In one embodiment, the mass ratio of the ferric salt, the ferrous salt, the precipitant, water and the oxidized carbon nanotubes is 2:1:(4-7):(18-36):(2-5).
[0010] In one embodiment, the oxidized carbon nanotubes have a diameter of 10 to 50 nm and a length of 5 to 10 μm.
[0011] In one embodiment, the viscosity of the vinyl silicone oil is in the range of 100 to 300 mPa·s; and / or,
[0012] The hydrogen content of the hydrogen-containing silicone oil is 0.6-2.0%.
[0013] In one embodiment, the ferric iron salt comprises at least one of ferric chloride, ferric sulfate and ferric nitrate; and / or,
[0014] The divalent iron salt includes at least one of ferrous chloride and ferrous sulfate; and / or,
[0015] The precipitant includes at least one of concentrated ammonia water, sodium hydroxide, potassium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.
[0016] In one embodiment, in step S10, the temperature for the coprecipitation reaction is 100-150° C.; and / or,
[0017] The coprecipitation reaction time is 3 to 6 hours.
[0018] In one embodiment, in step S10, the pH value of the coprecipitation reaction is 10-13.
[0019] In one embodiment, in step S20, the magnetic field strength is 0.5 to 1.0 T; and / or,
[0020] The mixture is placed in the magnetic field for 0.5 to 2 hours.
[0021] In one embodiment, in step S20, the temperature of thermal curing is 50-80° C.; and / or,
[0022] The thermal curing time is 0.5 to 3 hours.
[0023] The present invention provides a heat-conducting and wave-absorbing material, and the heat-conducting and wave-absorbing material comprises the heat-conducting and wave-absorbing material prepared by the preparation method.
[0024] The technical solution of the present invention provides a preparation method of a thermal conductive wave absorbing material, wherein the preparation method uses ferroferric oxide to modify oxidized carbon nanotubes to obtain magnetic oxidized carbon nanotubes, and the magnetic oxidized carbon nanotubes are oriented and arranged under the action of a magnetic field, which can greatly exert the thermal conductivity of carbon nanotubes and significantly improve the thermal conductivity of the material under a lower filling ratio; since ferroferric oxide also has wave absorbing properties, the prepared material has both thermal conductive properties and wave absorbing properties. The thermal conductive wave absorbing material prepared by the present invention can overcome the defects of the limited addition ratio of thermal conductive fillers and wave absorbing fillers in the preparation process of existing thermal conductive wave absorbing materials, and the mutual inhibition of thermal conductive properties and wave absorbing properties, and does not affect the mechanical properties of the original material after curing, so it can be used to solve the problems of the existing thermal conductive wave absorbing materials that the thermal conductive properties and wave absorbing properties cannot be taken into account and the mechanical properties are poor. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0026] Figure 1 This is a SEM electron microscope morphology image of the thermal conductive wave absorbing material in Example 2 of the present invention;
[0027] Figure 2 This is a SEM electron microscope element analysis diagram of the thermal conductive and wave absorbing material in Example 2 of the present invention.
[0028] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0031] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if "and / or" or "and / or" appears in the full text, its meaning includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0032] In recent years, the size of electronic devices represented by semiconductor components has become smaller and smaller, and the heat generation has continued to increase. At the same time, the accompanying electromagnetic interference problem has become more and more serious. The use of thermal conductive and absorbing materials can effectively reduce the operating temperature of electronic components, while reducing or shielding the electromagnetic noise generated by them. The overall research and development ideas of thermal conductive and absorbing materials are roughly the same, that is, adding functional fillers to the polymer matrix to make the material have thermal conductivity or wave absorption functions. Generally, by mixing traditional thermal conductive fillers and absorbers into the matrix material, a material with both thermal conductivity and wave absorption functions is obtained. However, since there is an upper limit to the total amount of functional fillers added to matrix materials such as rubber, the increase in the amount of a certain (thermal conductive, wave absorbing) filler added will inevitably lead to a decrease in the amount of another functional filler added, which makes the thermal conductivity and wave absorption properties of the thermal conductive and absorbing materials contradictory, and it is difficult to achieve the simultaneous improvement of the thermal conductivity and wave absorption properties of the material.
[0033] At present, the research and development of thermal conductive and wave absorbing materials can only balance the thermal conductivity and wave absorption performance indicators of the materials by comprehensively coordinating the addition ratio of the two fillers. It cannot meet the requirements of sensitive electronic devices for materials with both electromagnetic wave absorption function and efficient heat conduction ability.
[0034] In view of the problem that traditional dual-functional filler thermal conductive and wave absorbing composite materials require high filling of thermal conductors and absorbers at the same time, which will lead to a significant decrease in the mechanical properties of the composite materials, the market hopes to develop a single powder material with both thermal conductivity and wave absorbing dual functions for use in the preparation of thermal conductive and wave absorbing composite materials.
[0035] In view of this, the present invention proposes a method for preparing a thermal conductive wave absorbing material, comprising the following steps:
[0036] S10, mixing a trivalent iron salt, a divalent iron salt, a precipitant, water and oxidized carbon nanotubes to perform a coprecipitation reaction to obtain magnetic oxidized carbon nanotubes;
[0037] S20, mixing magnetic oxidized carbon nanotubes, vinyl silicone oil, and hydrogen-containing silicone oil to obtain a mixture, placing the mixture in a magnetic field to orient the magnetic oxidized carbon nanotubes along the direction of the magnetic field, and thermally curing the mixture after the orientation is completed to obtain a thermal conductive wave absorbing material;
[0038] Wherein, the mass ratio of the magnetic oxidized carbon nanotubes, vinyl silicone oil and hydrogen-containing silicone oil is (10-30): (50-100): (0.4-1.5).
[0039] The technical solution of the present invention provides a method for preparing a thermally conductive and absorbing material. The preparation method modifies oxidized carbon nanotubes by ferroferric oxide to obtain magnetic oxidized carbon nanotubes, and aligns the magnetic oxidized carbon nanotubes in a directional manner under the action of a magnetic field, which can greatly exert the thermal conductivity of carbon nanotubes and significantly improve the thermal conductivity of the material under a lower filling ratio. Since ferroferric oxide also has absorbing properties, the prepared material has both thermal conductivity and absorbing properties. The thermally conductive and absorbing material prepared by the present invention can overcome the defects of limited addition ratios of thermally conductive fillers and absorbing fillers in the preparation process of thermally conductive and absorbing materials, and mutual inhibition of thermal conductivity and absorbing properties, and does not affect the mechanical properties of the original material after curing. Therefore, it can be used to solve the problems of poor mechanical properties and inability to balance thermal conductivity and absorbing properties in existing thermally conductive and absorbing materials.
[0040] It should be noted that the oxidized carbon nanotubes in step S10 can be purchased or prepared by oneself. In the technical solution of the present application, the preparation method of preparing by oneself is:
[0041] A mixture of concentrated sulfuric acid and concentrated nitric acid was added to the carbon nanotubes, and the mixture was allowed to stand for 6 hours, and then filtered and dried to obtain oxidized carbon nanotubes;
[0042] Wherein, the volume ratio of the concentrated sulfuric acid to the concentrated nitric acid is 3:1 to 1:3.
[0043] In an embodiment of the present invention, the mass ratio of the ferric iron salt, the divalent iron salt, the precipitant, water and the oxidized carbon nanotubes is 2:1:(4-7):(18-36):(2-5). The ferric iron salt and the divalent iron salt are mixed in a certain proportion, and the precipitant (OH - ), stirring the reaction to obtain magnetic ferroferric oxide. The surface of the oxidized carbon nanotubes obtained by acidification has hydroxyl functional groups (-OH), and ferric iron salt, divalent iron salt, precipitant, water and oxidized carbon nanotubes are subjected to coprecipitation reaction to obtain ferroferric oxide-modified oxidized carbon nanotubes. Setting the mass ratio of ferric iron salt, divalent iron salt, precipitant, water and oxidized carbon nanotubes within the above range is conducive to balancing thermal conductivity and wave absorption performance, and obtaining a material with excellent thermal conductivity and wave absorption performance.
[0044] In an embodiment of the present invention, the diameter of the oxidized carbon nanotubes is 10 to 50 nm, and the length is 5 to 10 μm. The diameter and length of the oxidized carbon nanotubes will affect their thermal conductivity. Generally speaking, the larger the diameter and length, the better the thermal conductivity. However, further increasing the diameter and length will affect the modification and dispersion of the carbon nanotubes. Selecting an oxidized carbon nanotube with a diameter of 10 to 50 nm and a length of 5 to 10 μm is conducive to improving the thermal conductivity of the obtained thermal conductive wave absorbing material, and improving the dispersion and sorting of the oxidized carbon nanotubes in the obtained thermal conductive wave absorbing material.
[0045] In the embodiment of the present invention, the viscosity of the vinyl silicone oil is in the range of 100 to 300 mPa·s. Setting the viscosity of the vinyl silicone oil in the above range is beneficial to adjusting the hardness of the final product and prolonging the operation time.
[0046] In an embodiment of the present invention, the hydrogen content of the hydrogen-containing silicone oil is 0.6-2.0%. The hydrogen content of the hydrogen-containing silicone oil within the above range is beneficial to prolonging the operation time and improving the dispersion performance of the thermal conductive and wave absorbing material.
[0047] In an embodiment of the present invention, the hydrogen-containing silicone oil includes at least one of MH series hydrogen-containing silicone oil of Silicone Technology, Dow Corning MHX-1107, and Shin-Etsu KF99.
[0048] In an embodiment of the present invention, the ferric iron salt includes at least one of ferric chloride, ferric sulfate and ferric nitrate.
[0049] In an embodiment of the present invention, the divalent iron salt includes at least one of ferrous chloride and ferrous sulfate.
[0050] In an embodiment of the present invention, the precipitant includes at least one of concentrated ammonia water, sodium hydroxide, potassium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide. Concentrated ammonia water is preferably used as the precipitant.
[0051] In an embodiment of the present invention, in step S10, the temperature for the coprecipitation reaction is 100-150°C, and the time for the coprecipitation reaction is 3-6 hours. The temperature, time, and pH value of the reaction will affect the performance and structure of the magnetic material obtained by the coprecipitation method. Setting the time and temperature of the coprecipitation reaction within this range is conducive to obtaining a composite material with a balance between thermal conductivity and wave absorption performance.
[0052] In an embodiment of the present invention, in step S10, the pH value of the coprecipitation reaction is 10 to 13. Selecting the pH of the coprecipitation reaction within this range is conducive to obtaining a composite material with balanced thermal conductivity and microwave absorption properties.
[0053] In an embodiment of the present invention, in step S20, the magnetic field strength is 0.5 to 1.0 T, and the mixture is placed in the magnetic field for 0.5 to 3 hours. The magnetic field strength is related to the time required for directional sorting, and the stronger the magnetic field strength, the shorter the time required for directional sorting, and the better the sorting state.
[0054] In an embodiment of the present invention, the temperature for heat curing is 50-80° C., and the time for heat curing is 0.5-3 hours. The curing parameters will affect the mechanical properties of the material. Selecting the temperature and time for heat curing within the above range is conducive to obtaining a composite material with excellent mechanical properties.
[0055] The present invention provides a heat-conducting and wave-absorbing material, and the heat-conducting and wave-absorbing material comprises the heat-conducting and wave-absorbing material prepared by the preparation method.
[0056] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0057] Example 1
[0058] A method for preparing a heat-conducting and wave-absorbing material comprises the following steps:
[0059] (1) Weigh 100 g of carbon nanotubes, add 500 mL of concentrated sulfuric acid and 500 mL of concentrated nitric acid, let stand for 6 hours, filter and dry to obtain oxidized carbon nanotubes (the diameter of the oxidized carbon nanotubes is 10 to 20 nm and the length is 8 to 10 μm).
[0060] (2) In a three-necked flask, 10 g of oxidized carbon nanotubes and 100 mL of deionized water were added, followed by the addition of 10.8 g of FeCl3·6H2O and 5.56 g of FeSO4·7H2O. The mixture was stirred at 500 r / min for 10 min and then heated to 60°C. 25 mL of concentrated ammonia was slowly added dropwise and the mixture was stirred for 20 min. Stirring was stopped when the mixture was heated to 80°C and aged for 20 min. 80 mL of the aged solution was transferred to a 100 mL hydrothermal reactor and subjected to hydrothermal reaction at 145°C for 6 h (the pH value during the reaction was 10-13). After the reaction was completed, the mixture was cooled to room temperature to obtain magnetic oxidized carbon nanotubes (oxidized carbon nanotubes modified with ferroferric oxide).
[0061] (3) 15 g of ferroferric oxide-modified carbon nanotubes, 50 g of vinyl silicone oil (viscosity of 100 mPa·s), and 1.5 g of hydrogen-containing silicone oil (hydrogen content of 0.6%) were mixed and oriented in a magnetic field with a strength of 0.5 T for 2 h. After the orientation was completed, the mixture was heated and cured at 60° C. for 1 h to obtain a thermal conductive and wave-absorbing material.
[0062] Example 2
[0063] This example follows a method similar to that of Example 1, except that in step (2), the oxidized carbon nanotubes are 30 g, deionized water is 200 mL, FeCl3·6H2O is 10.8 g, FeSO4·7H2O is 5.56 g, and concentrated ammonia is 45 mL, and the hydrothermal reaction is carried out at 120°C for 3 h; in step (3), the oxidized carbon nanotubes modified with ferrosoferric oxide are 30 g, the vinyl silicone oil is 60 g, and the hydrogen-containing silicone oil is 1.0 g, the magnetic field strength is 0.8 T, the time of being placed in the magnetic field is 1 h, the heating curing temperature is 55°C, the heating curing is for 1 h, the viscosity of the vinyl silicone oil is 200 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 1.2%.
[0064] Example 3
[0065] This example is carried out in a manner similar to that of Example 1, except that in step (2), the oxidized carbon nanotubes are 15 g, deionized water is 100 mL, FeCl3·6H2O is 5.4 g, FeSO4·7H2O is 2.78 g, and concentrated aqueous ammonia is 15 mL, and the hydrothermal reaction is carried out at 110° C. for 6 h; in step (3), the oxidized carbon nanotubes modified with ferrosoferric oxide are 10 g, the vinyl silicone oil is 100 g, and the hydrogen-containing silicone oil is 0.4 g, the magnetic field strength is 1.0 T, the time of being placed in the magnetic field is 2 h, the heating curing temperature is 80° C., and the heating curing is carried out for 3 h; the viscosity of the vinyl silicone oil is 300 mPa·s, and the hydrogen content of the hydrogen-containing silicone oil is 2.0%.
[0066] Example 4
[0067] This embodiment follows a method similar to that of embodiment 2, except that the diameter of the oxidized carbon nanotubes is 30-50 nm and the length is 5-8 μm.
[0068] Example 5
[0069] This example follows a method similar to that of Example 2, except that ferric sulfate is used as the ferric salt and ferrous chloride is used as the ferrous salt.
[0070] Example 6
[0071] This example follows a method similar to that of Example 2, except that sodium hydroxide is used as the precipitant.
[0072] Comparative Example 1
[0073] Compared with Example 2, step (1) is not performed, and in step (2), carbon nanotubes are used instead of oxidized carbon nanotubes for the hydrothermal reaction. The rest is the same as Example 2.
[0074] Comparative Example 2
[0075] Compared with Example 2, step (1) and step (2) are not performed, and in step (3), carbon nanotubes are used instead of oxidized carbon nanotubes modified with ferrosoferric oxide. The rest is the same as Example 2.
[0076] Comparative Example 3
[0077] Compared with Example 2, the mass ratio of the oxidized carbon nanotubes modified with ferrosoferric oxide, silicone oil, and hydrogen-containing silicone oil in step (3) is 25:100:3, and the rest is the same as Example 2.
[0078] Performance Testing
[0079] The microstructure, thermal conductivity and absorbing performance of the thermal conductive absorbing materials prepared in Examples 1-6 and Comparative Examples 1-3 were tested in the following specific steps:
[0080] Microstructure observation: SEM electron microscope analysis was performed on the thermal conductive wave absorbing material of Example 2. 0.1g of the thermal conductive wave absorbing material was placed on the conductive glue, placed in a vacuum chamber, and the magnification was adjusted to perform scanning electron microscope photography. The SEM electron microscope morphology is shown in the figure. Figure 1 As shown in the elemental analysis diagram Figure 2 As shown. Figure 1 It can be seen that spherical iron oxide is grafted on the carbon nanotubes, and elemental analysis also shows that there are carbon, oxygen, iron, etc. ( Figure 2 ), indicating that the material was successfully prepared.
[0081] Thermal conductivity test: Thermal conductivity is evaluated by thermal conductivity. The larger the thermal conductivity, the better the thermal conductivity. The thermal conductivity is tested according to the standard GB / T 29313-2012, and the test results are shown in Table 1.
[0082] Wave absorption performance test: The wave absorption performance is tested in accordance with GJB 5239-2004. The specific method is to prepare the above materials into 2mm gaskets for testing, and use the effective absorption bandwidth to express it. If the reflection loss is less than -10dB, it means that the material absorbs 90% of the electromagnetic energy, which is called effective absorption; the frequency range where the reflection loss is less than -10dB is called the effective absorption bandwidth; the smaller the reflection loss of the absorbing material and the larger the span of the effective absorption bandwidth, the better the wave absorption performance of the material. The test results are shown in Table 1.
[0083] Mechanical properties test: Hardness is used to express mechanical properties, and the hardness test method is carried out according to GB / T 2411-2008. The test results are shown in Table 1.
[0084] Table 1 Performance test results of thermal conductive wave absorbing materials of Examples 1-6 and Comparative Examples 1-3
[0085]
[0086] It can be seen from Table 1 that, compared with the materials of Comparative Examples 1-3 and the existing thermal conductive wave absorbing materials, the thermal conductive wave absorbing materials of Examples 1-6 have good thermal conductivity, wave absorbing performance and mechanical properties.
[0087] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a thermally conductive and wave-absorbing material, characterized in that: The following steps are involved: S10, mixing a trivalent iron salt, a divalent iron salt, a precipitant, water and oxidized carbon nanotubes to perform a coprecipitation reaction to obtain magnetic oxidized carbon nanotubes; S20, mixing magnetic oxidized carbon nanotubes, vinyl silicone oil, and hydrogen-containing silicone oil to obtain a mixture, placing the mixture in a magnetic field to orient the magnetic oxidized carbon nanotubes along the direction of the magnetic field, and thermally curing the mixture after the orientation is completed to obtain a thermal conductive wave absorbing material; Wherein, the mass ratio of the magnetic oxidized carbon nanotubes, vinyl silicone oil and hydrogen-containing silicone oil is (10-30): (50-100): (0.4-1.5).
2. The method for preparing the thermal conductive wave absorbing material according to claim 1, characterized in that: The mass ratio of the ferric iron salt, the ferrous iron salt, the precipitant, water and the oxidized carbon nanotubes is 2:1:(4-7):(18-36):(2-5).
3. The method for preparing the thermal conductive and wave absorbing material according to claim 1, characterized in that: The diameter of the oxidized carbon nanotubes is 10-50 nm, and the length is 5-10 μm.
4. The method for preparing the thermal conductive and wave absorbing material according to claim 1, characterized in that: The viscosity of the vinyl silicone oil is in the range of 100 to 300 mPa·s; and / or, The hydrogen content of the hydrogen-containing silicone oil is 0.6-2.0%.
5. The method for preparing the thermal conductive and wave absorbing material according to claim 1, characterized in that: The ferric iron salt comprises at least one of ferric chloride, ferric sulfate and ferric nitrate; and / or, The divalent iron salt includes at least one of ferrous chloride and ferrous sulfate; and / or, The precipitant includes at least one of concentrated ammonia water, sodium hydroxide, potassium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.
6. The method for preparing the thermal conductive and wave absorbing material according to claim 1, characterized in that: In step S10, the temperature for the coprecipitation reaction is 100-150° C.; and / or, The coprecipitation reaction time is 3 to 6 hours.
7. The method for preparing the thermal conductive and wave absorbing material according to claim 1, characterized in that: In step S10, the pH value of the coprecipitation reaction is 10-13.
8. The method for preparing the thermal conductive and wave absorbing material according to claim 1, characterized in that: In step S20, the magnetic field strength is 0.5 to 1.0 T; and / or, The mixture is placed in the magnetic field for 0.5 to 2 hours.
9. The method for preparing a thermal conductive wave absorbing material according to claim 1, characterized in that: In step S20, the temperature of thermal curing is 50-80° C.; and / or, The thermal curing time is 0.5 to 3 hours.
10. A thermal conductive wave absorbing material, characterized in that: The thermal conductive wave absorbing material comprises the thermal conductive wave absorbing material prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparing ferroferric oxide / carbon nano tube composite material
CN102583315A
Heat-conducting wave-absorbing silica gel composite material and preparation method thereof
CN112194903A
Preparation method of Fe3O4@MWCNTs nano composite material and electronic equipment
CN113999432A