Carbon-based composite shaped filter material capable of prolonging service life of engine oil and preparation method of carbon-based composite shaped filter material
By functional modification of carbon materials and polyurethane insertion microfoam composite molding, carbon-based composite filter materials with microfoam structure are prepared, which solves the problems of fast decay and short service life of engine oil, and realizes efficient purification and use of engine oil Extended lifespan.
Patent Information
- Application Number
- CN202410953145.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-26
AI Technical Summary
During use, the existing engine oil filter materials have rapid decay due to oxidation and decomposition, short service life, and the filtration accuracy and purification performance need to be improved.
Functional compounds are used to modify the carbon material and compositely shape it with polyurethane insertion microfoam to prepare carbon-based composite shaped filter material with microfoam structure to achieve the triple effect of sustained release-adsorption-filtration, and dynamic supplementary function Compounds that delay engine oil decay and efficiently purify pollutants.
Through the physical, chemical adsorption of carbon materials and the filtration of microfoam structure, the service life of the engine oil is significantly extended, the oil purification performance is improved, the oil decay failure is delayed, and the engine operation is ensured.
Smart Images

Figure CN119020063A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of activated carbon material application and engine oil filtration, and specifically relates to a carbon-based composite shaped filter material for extending the service life of engine oil and a preparation method thereof. Background Art
[0002] Engine oil has the functions of reducing friction, reducing erosion and sealing, ensuring the normal and stable operation of the engine. Engine oil is mainly composed of base oil and additives. During use, it is decomposed, oxidized, consumed, and produces pollutants such as organic acids and colloids. At the same time, it also produces metal grinding chips, dust, carbon deposits, etc. due to the engine, resulting in an increase in the impurity content of the engine oil and a decrease in quality. New engine oil needs to be replaced to meet the use requirements of the engine. According to statistics, the amount of waste lubricating oil generated in my country is about 8 million tons per year. Therefore, it is of great significance to extend the service life of engine oil.
[0003] Adding different additives to the base oil, such as antioxidants, anti-wear agents, dispersants, etc., can produce composite engine oil, which can effectively improve the quality and service life of the engine oil. At present, composite engine oil is obtained by homogenizing and mixing base oil and additives. Since the additives are added to the base oil in full at one time, when the engine is in working condition, the additives are fully involved in the operation and reaction, resulting in fast consumption and poor sustainability of the effect. The decay of composite engine oil becomes more and more significant with the extension of time, which greatly affects its service life. The filter can filter out colloidal sediments, carbon deposits, metal debris and other pollutants in the engine oil, thereby keeping the engine oil clean and helping to extend the service life of the engine oil. As the use time increases, the pollutants and impurities in the engine oil gradually increase, resulting in its acid value, alkalinity value, moisture, fuel dilution, viscosity and other indicators not meeting the engine's use requirements. The engine oil and its corresponding filter must be replaced to ensure the normal operation of the engine.
[0004] A carbon-based shaped engine oil purification material with a special mesh structure is prepared by bonding activated carbon and a polymer adhesive. The material has good purification performance, large engine oil flux, and wide adaptability (CN114699846A). However, since the filtering effect of the carbon-based shaped purification filter material is mainly generated by the woven mesh and channel structure, its filtering accuracy and purification performance need to be further improved. At the same time, during the use of engine oil, due to the high temperature, high pressure, high shear force and other working conditions of the engine, the additives in the engine oil are consumed due to oxidation, decomposition, etc., resulting in rapid decay of the engine oil and reduced quality. The decay and failure of the engine oil and the increase of pollutants lead to its poor quality and short service life, and it needs to be replaced to meet the requirements of engine use. Summary of the invention
[0005] In view of the problems of fast oil decay and short service life of existing filter materials, one technical problem to be solved by the present invention is to provide a method for preparing a carbon-based composite shaped filter material that can extend the service life of engine oil. A carbon-based composite shaped filter element that can extend the service life of engine oil is prepared by selecting a variety of functional compounds, functionalizing and modifying carbon materials, and composite shaping with polyurethane intercalation micro-foaming. Another technical problem to be solved by the present invention is to provide a carbon-based composite shaped filter material that can extend the service life of engine oil. The purification material has the triple effect of "slow release-adsorption-filtration". Its slow release characteristics can dynamically supplement functional compounds, extend the synergistic effects of functional compounds such as anti-oxidation and anti-wear, and effectively delay the decay and failure of engine oil. The physical and chemical adsorption of carbon materials and the filtering effect of micro-foam structure can efficiently purify engine oil pollutants. The service life of engine oil is extended by delaying the decay of engine oil and efficiently purifying and removing pollutants.
[0006] Technical solution: In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a carbon-based composite shaped filter material for extending the service life of engine oil comprises the following steps: functionalizing a carbon material with a functional compound to obtain a functionalized carbon material; then the carbon-based composite shaped filter material is prepared by inserting and micro-foaming composite shaping with polyurethane; the functional compound is composed of an amine antioxidant, a phenolic antioxidant and an anti-wear additive; and the carbon-based composite shaped filter material has a micro-foam structure.
[0008] The preparation method of the carbon-based composite shaped filter material for extending the service life of engine oil is as follows: three types of functional compounds are respectively compositely enriched and modified with carbon materials to obtain amine antioxidant modified carbon materials, phenol antioxidant modified carbon materials and anti-wear modified carbon materials; the functionalized carbon material is prepared by mixing amine antioxidant modified carbon materials, phenol antioxidant modified carbon materials and anti-wear modified carbon materials, and the proportions are 20% to 30%, 50% to 60%, and 10% to 30%, respectively, and the sum of the weight percentages of the three types of modified carbon materials is 100%; preferably, the proportions are 20% to 30%, 50% to 60%, and 10% to 25%, respectively; further preferably, the proportions are 30%, 50%, and 20%, respectively.
[0009] The preparation method of the carbon-based composite shaped filter material for extending the service life of engine oil, the content of amine antioxidants in the amine antioxidant modified carbon material is 1% to 3%, the content of phenolic antioxidants in the phenolic antioxidant modified carbon material is 1% to 5%, and the content of anti-wear additives in the anti-wear modified carbon material is 1% to 5%; preferably, the content of amine antioxidants in the amine antioxidant modified carbon material is 1% to 3%, the content of phenolic antioxidants in the phenolic antioxidant modified carbon material is 1.5% to 5%, and the content of anti-wear additives in the anti-wear modified carbon material is 3% to 5%.
[0010] The method for preparing a carbon-based composite shaped filter material for extending the service life of engine oil, wherein the amine antioxidant is one of N,N'-dimethyl-p-phenylenediamine or N,N'-diphenyl-p-phenylenediamine or a mixture of two thereof; the phenolic antioxidant is one of 2,6-di-tert-butylphenol or 2,6-di-tert-butyl-4-methylphenol or a mixture of two thereof; the anti-wear additive is one of tricresyl phosphate or tricresyl phosphate or a mixture of two thereof; preferably, the amine antioxidant is a mixture of N,N'-dimethyl-p-phenylenediamine and N,N'-diphenyl-p-phenylenediamine, with a mass ratio of 0.6:1-1.5:1, and / or the phenolic antioxidant is 2,6-di-tert-butylphenol or 2,6-di-tert-butyl-4-methylphenol or a mixture of two thereof. A mixture of di-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol in a mass ratio of 1:1.5-1:1, and / or the anti-wear additive is a mixture of tricresyl phosphate and trixylene phosphate in a mass ratio of 1:2.4-1:1; further preferably, the amine antioxidant is a mixture of N,N'-dimethyl-p-phenylenediamine and N,N'-diphenyl-p-phenylenediamine in a mass ratio of 1.5:1, the phenolic antioxidant is a mixture of 2,6-di-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol in a mass ratio of 1:1.5, and the anti-wear additive is a mixture of tricresyl phosphate and trixylene phosphate in a mass ratio of 1:1.5.
[0011] In the method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil, the mass ratio of the functionalized carbon material to the polyurethane is 2:1 to 8:1; preferably, the mass ratio of the functionalized carbon material to the polyurethane is 3.3:1 to 5:1; further preferably, the mass ratio of the functionalized carbon material to the polyurethane is 4:1.
[0012] The preparation method of the carbon-based composite shaped filter material for extending the service life of engine oil, the polyurethane comprises component A and component B, component A is obtained by compounding polyether polyol, polyester polyol and auxiliary agent, component B is diphenylmethane diisocyanate; the auxiliary agent is organic tin or triethanolamine or a mixture of the two; preferably, the auxiliary agent is a mixture of organic tin and triethanolamine, and the mass ratio is 1:1.
[0013] The preparation method of the carbon-based composite shaped filter material for extending the service life of engine oil comprises a preparation process of inserting micro-foaming composite shaping, and the specific steps are: adding polyurethane component A to the functionalized carbon material at room temperature and mixing evenly; then adding polyurethane component B, stirring and reacting rapidly, the stirring speed is 300-1500r / min, and the time is 1-10min; then filling in a fixed mold and micro-foaming molding under controlled pressure at room temperature, the pressure is 0.1-1kg / cm 2 , time is 10 to 240 min; preferably, the stirring speed is 500 to 1000 r / min, the time is 3 to 7 min, and the pressure is 0.3 to 0.7 kg / cm 2, time is 60 to 200 min; more preferably, the stirring speed is 1000 r / min, the time is 3 min, and the pressure is 0.4 kg / cm 2 , time is 150min.
[0014] The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil comprises the following steps:
[0015] (1) An amine antioxidant is dissolved in ethanol to prepare a solution, and then ultrasonically impregnated with a carbon material, filtered, and vacuum dried to obtain an amine antioxidant modified carbon material; a phenolic antioxidant is dissolved in ethanol to prepare a solution, and then ultrasonically impregnated with a carbon material, filtered, and vacuum dried to obtain a phenolic antioxidant modified carbon material; an anti-wear modifier is dissolved in ethanol to prepare a solution, and then ultrasonically impregnated with a carbon material, filtered, and vacuum dried to obtain an anti-wear modified carbon material;
[0016] (2) Amine antioxidant modified carbon material, phenol antioxidant modified carbon material and anti-wear modified carbon material are mixed to obtain a functional modified carbon-based material;
[0017] (3) The polyurethane comprises A and B, polyester polyol and an auxiliary agent are added to the polyether polyol to obtain the polyurethane component A, wherein the auxiliary agent is organic tin or triethanolamine;
[0018] (4) adding the polyurethane component A obtained in step (3) to the functionalized carbon material after compounding in step (2), uniformly mixing at room temperature, then adding the polyurethane component B for rapid stirring and reaction, filling the mixture into a fixed mold for pressure-controlled micro-foaming at room temperature, and obtaining a carbon-based composite shaped filter material after demolding; the component B is diphenylmethane diisocyanate.
[0019] The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil comprises the following steps: the mass ratio of polyether polyol, polyester polyol and auxiliary agent is (2-5):1:(0.05-0.5); the mass ratio of component A to component B is 0.5:1-3:1; preferably, the mass ratio of polyether polyol, polyester polyol and auxiliary agent is (2-5):1:(0.05-0.4); the mass ratio of component A to component B is 0.8:1-1.2:1; further preferably, the mass ratio of polyether polyol, polyester polyol and auxiliary agent is 3.5:1:0.4; the mass ratio of component A to component B is 1:1.
[0020] The carbon-based composite shaped filter material prepared by the above method can prolong the service life of engine oil.
[0021] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0022] 1. The present invention is based on the fact that engine oil decays and fails and has a short service life due to changes in composition and consumption of additives due to thermal decomposition and oxidation under high temperature and high pressure during use. By selecting a variety of functional compounds and further compounding them with carbon materials, a modified carbon material with a sustained release effect is constructed. By exerting the synergistic effect of the various functional compounds on the anti-oxidation and anti-wear effects of the engine oil and the sustained release effect of the carbon material on the functional compounds, the functional compounds are dynamically sustained-released and supplemented during use, and the synergistic effect of the functional compounds is exerted, thereby effectively delaying the decay and failure of the engine oil and extending the service life of the engine oil.
[0023] 2. The present invention embeds the functionalized modified carbon material and the two-component polyurethane through micro-foaming and composite shaping, and forms a micro-foam structure with certain through holes between the carbon material particles. The porosity of the micro-foam structure ensures good oil flow. At the same time, the micro-foam is a three-dimensional structure with different sizes and arranged in various directions, which produces a huge specific surface area and pore volume, effectively improving the filtration efficiency and dirt holding capacity, improving the oil purification performance and extending the service life of the oil.
[0024] 3. The carbon-based composite shaped filter material for extending the service life of engine oil of the present invention has the triple effects of "slow release-adsorption-filtration". Dynamic slow release of functional compounds and synergistic effect of functional compounds delay the decay and failure of engine oil; the strong physical and chemical adsorption of carbon materials and the efficient filtering effect of micro-foam structure and large dirt holding capacity realize efficient and long-term engine oil purification. The carbon-based composite shaped filter material extends the service life of engine oil through the combined effects of slow release, adsorption and filtration.
[0025] 4. The carbon-based composite shaped filter material of the present invention is a body-shaped deep filter medium with a porosity of more than 30% and a pore volume of more than 3.0*10 6 mm 3 The diameter of the micro-foam structure is 20 to 100 μm; it is encapsulated into a carbon-based composite shaped filter. After 10,000 kilometers of actual vehicle operation, the change rate of engine oil kinematic viscosity (100°C) is less than 10%, the acid value increase is <1.0 mgKOH / g, the gasoline dilution is <0.7%, the iron content is <13 μg / g, and the silicon content is <15 μg / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a diagram of the body structure of the carbon-based composite shaped filter material in Example 5 and the micro-foam structure formed between the carbon material particles. DETAILED DESCRIPTION
[0027] The present invention is further illustrated below in conjunction with specific examples. The examples are implemented based on the technical solutions of the present invention. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0028] The content of the functional compound in the modified carbon material disclosed in the present invention is determined by a weight method; the porosity and pore volume of the carbon-based composite shaped filter material are tested by CT scanning; and the micro-foam structure of the carbon-based composite shaped filter material is analyzed by a scanning electron microscope.
[0029] Example 1
[0030] A method for preparing a carbon-based composite shaped filter material for extending the service life of engine oil comprises the following steps:
[0031] (1) Select N,N'-dimethyl-p-phenylenediamine and N,N'-diphenyl-p-phenylenediamine in a mass ratio of 1:1 and dissolve them in ethanol to prepare a solution, add carbon material, and filter, wash, and vacuum dry after ultrasonic impregnation to obtain an amine antioxidant modified carbon material with an amine antioxidant content of 1.5%; select 2,6-di-tert-butylphenol and 2,6-di-tert-butyl-4-methylphenol in a mass ratio of 1:1 and dissolve them in ethanol to prepare a solution, add carbon material, and filter, wash, and vacuum dry after ultrasonic impregnation to obtain a phenol antioxidant modified carbon material with a phenol antioxidant content of 2.0%; select tricresyl phosphate and tricresyl phosphate in a mass ratio of 1:1 and dissolve them in ethanol to prepare a solution, add carbon material, and filter, wash, and vacuum dry after ultrasonic impregnation to obtain an anti-wear modified carbon material with an anti-wear additive content of 3.5%;
[0032] (2) Amine antioxidant modified carbon material, phenol antioxidant modified carbon material and anti-wear modified carbon material are uniformly mixed in the ratio of 25%, 55% and 20% to obtain a functionalized carbon material;
[0033] (3) adding polyester polyol and organotin into polyether polyol to prepare polyurethane component A. The mass ratio of polyether polyol, polyester polyol and organotin is 2:1:0.1;
[0034] (4) At room temperature, 20 g of the polyurethane component A of step (3) was added to 200 g of the functionalized carbon material of step (2), and the mixture was uniformly mixed for 2 min. Then, 25 g of the polyurethane component B was added, and the mixture was reacted at a stirring speed of 1000 r / min for 3 min. The mixture was filled in a fixed mold at a pressure of 0.3 kg / cm 2 The micro-foaming was performed for 200 minutes, and the carbon-based composite shaped filter material was obtained after demoulding.
[0035] The porosity of the carbon-based composite filter material is 32.35%, and the pore volume is 3.37*10 6 mm 3 The diameter of the microfoam structure is 20 to 80 μm.
[0036] Example 2
[0037] A method for preparing a carbon-based composite shaped filter material for extending the service life of engine oil comprises the following steps:
[0038] (1) N, N'-dimethyl-p-phenylenediamine was dissolved in ethanol to prepare a solution, and a carbon material was added. After ultrasonic impregnation, the solution was filtered, washed, and vacuum dried to obtain an amine antioxidant modified carbon material with an amine antioxidant content of 1.7%; 2, 6-di-tert-butylphenol and 2, 6-di-tert-butyl-4-methylphenol were dissolved in ethanol in a mass ratio of 4:6 to prepare a solution, and a carbon material was added. After ultrasonic impregnation, the solution was filtered, washed, and vacuum dried to obtain a phenol antioxidant modified carbon material with a phenol antioxidant content of 2.5%; trixylene phosphate was dissolved in ethanol to prepare a solution, and a carbon material was added. After ultrasonic impregnation, the solution was filtered, washed, and vacuum dried to obtain an anti-wear modified carbon material with an anti-wear additive content of 3.5%;
[0039] (2) Amine antioxidant modified carbon material, phenol antioxidant modified carbon material and anti-wear modified carbon material are uniformly mixed in the ratio of 20%, 55% and 25% to obtain a functionalized carbon material;
[0040] (3) adding polyester polyol and triethanolamine to polyether polyol to prepare polyurethane component A; the mass ratio of polyether polyol, polyester polyol and triethanolamine is 4:1:0.1;
[0041] (4) At room temperature, 20 g of the polyurethane component A of step (3) was added to 200 g of the functionalized carbon material of step (2), and the mixture was uniformly mixed for 2 min. Then, 20 g of the polyurethane component B was added, and the mixture was reacted at a stirring speed of 700 r / min for 3 min. The mixture was filled in a fixed mold at a pressure of 0.7 kg / cm 2 The product was micro-foamed and shaped for 60 minutes, and the carbon-based composite shaped filter material was obtained after demoulding.
[0042] The porosity of the carbon-based composite filter material is 31.07%, and the pore volume is 3.03*10 6 mm 3 The diameter of the microfoam structure is 30 to 90 μm.
[0043] Example 3
[0044] A method for preparing a carbon-based composite shaped filter material for extending the service life of engine oil comprises the following steps:
[0045] (1) N, N'-dimethyl-p-phenylenediamine is dissolved in ethanol to prepare a solution, a carbon material is added, and the solution is filtered, washed, and vacuum dried after ultrasonic impregnation to obtain an amine antioxidant modified carbon material, wherein the amine antioxidant content is 2.0%; 2, 6-di-tert-butyl-4-methylphenol is dissolved in ethanol to prepare a solution, a carbon material is added, and the solution is filtered, washed, and vacuum dried to obtain a phenol antioxidant modified carbon material, wherein the phenol antioxidant content is 2.5%; tricresyl phosphate is dissolved in ethanol to prepare a solution, a carbon material is added, and the solution is filtered, washed, and vacuum dried after ultrasonic impregnation to obtain an anti-wear modified carbon material, wherein the anti-wear additive content is 3.8%;
[0046] (2) Amine antioxidant modified carbon material, phenol antioxidant modified carbon material and anti-wear modified carbon material are uniformly mixed in the ratio of 30%, 60% and 10% to obtain a functionalized carbon material;
[0047] (3) adding polyester polyol and triethanolamine to polyether polyol to prepare polyurethane component A; the mass ratio of polyether polyol, polyester polyol and triethanolamine is 3:1:0.05;
[0048] (4) At room temperature, 30 g of the polyurethane component A of step (3) was added to 200 g of the functionalized carbon material of step (2), and the mixture was uniformly mixed for 2 min. Then, 25 g of the polyurethane component B was added, and the mixture was reacted at a stirring speed of 500 r / min for 7 min. The mixture was filled in a fixed mold at a pressure of 0.7 kg / cm 2 The micro-foaming was performed for 90 minutes, and the carbon-based composite shaped filter material was obtained after demoulding.
[0049] The porosity of the carbon-based composite filter material is 30.59% and the pore volume is 3.02*10 6 mm 3 , the diameter of the microfoam structure is 30 to 100 μm.
[0050] Example 4
[0051] A method for preparing a carbon-based composite shaped filter material for extending the service life of engine oil comprises the following steps:
[0052] (1) Select N, N'-dimethyl-p-phenylenediamine and N, N'-diphenyl-p-phenylenediamine in a mass ratio of 4:6 and dissolve in ethanol to prepare a solution, add carbon material, and filter, wash, and vacuum dry after ultrasonic impregnation to obtain an amine antioxidant modified carbon material with an amine antioxidant content of 1.0%; select 2, 6-di-tert-butylphenol and 2, 6-di-tert-butyl-4-methylphenol in a mass ratio of 1:1 and dissolve in ethanol to prepare a solution, add carbon material, and filter, wash, and vacuum dry after ultrasonic impregnation to obtain a phenol antioxidant modified carbon material with a phenol antioxidant content of 1.5%; select tricresyl phosphate and tricresyl phosphate in a mass ratio of 3:7 and dissolve in ethanol to prepare a solution, add carbon material, and filter, wash, and vacuum dry after ultrasonic impregnation to obtain an anti-wear modified carbon material with an anti-wear additive content of 3.0%;
[0053] (2) Amine antioxidant modified carbon material, phenol antioxidant modified carbon material and anti-wear modified carbon material are uniformly mixed in the ratio of 30%, 50% and 20% to obtain a functionalized carbon material;
[0054] (3) adding polyester polyol and organotin into polyether polyol to prepare polyurethane component A; the mass ratio of polyether polyol, polyester polyol and organotin is 5:1:0.05;
[0055] (4) At room temperature, 30 g of the polyurethane component A of step (3) was added to 200 g of the functionalized carbon material of step (2), and the mixture was uniformly mixed for 2 min. Then, 30 g of the polyurethane component B was added, and the mixture was reacted at a stirring speed of 700 r / min for 5 min. The mixture was filled in a fixed mold at a pressure of 0.5 kg / cm 2 The micro-foaming was performed for 200 minutes, and the carbon-based composite shaped filter material was obtained after demoulding.
[0056] After testing, the porosity of the carbon-based composite filter material is 33.62%, and the pore volume is 3.31*10 6 mm 3 The diameter of the microfoam structure is 30 to 60 μm.
[0057] Example 5
[0058] A method for preparing a carbon-based composite shaped filter material for extending the service life of engine oil comprises the following steps:
[0059] (1) Select N, N'-dimethyl-p-phenylenediamine and N, N'-diphenyl-p-phenylenediamine in a mass ratio of 6:4 and dissolve them in ethanol to prepare a solution, add carbon material, and filter, wash, and vacuum dry after ultrasonic impregnation to obtain an amine antioxidant modified carbon material with an amine antioxidant content of 3.0%; select 2, 6-di-tert-butylphenol and 2, 6-di-tert-butyl-4-methylphenol in a mass ratio of 4:6 and dissolve them in ethanol to prepare a solution, add carbon material, and filter, wash, and vacuum dry after ultrasonic impregnation to obtain a phenol antioxidant modified carbon material with a phenol antioxidant content of 5.0%; select tricresyl phosphate and tricresyl phosphate in a mass ratio of 4:6 and dissolve them in ethanol to prepare a solution, add carbon material, and filter, wash, and vacuum dry after ultrasonic impregnation to obtain an anti-wear modified carbon material with an anti-wear additive content of 5.0%;
[0060] (2) Amine antioxidant modified carbon material, phenol antioxidant modified carbon material and anti-wear modified carbon material are uniformly mixed in the ratio of 30%, 50% and 20% to obtain a functionalized carbon material;
[0061] (3) adding polyester polyol and auxiliary agents, organotin and triethanolamine (mass ratio 1:1) to polyether polyol to obtain polyurethane component A; the mass ratio of polyether polyol, polyester polyol and auxiliary agent is 3.5:1:0.4;
[0062] (4) At room temperature, 25 g of the polyurethane component A of step (3) was added to 200 g of the functionalized carbon material of step (2), and the mixture was uniformly mixed for 2 min. Then, 25 g of the polyurethane component B was added, and the mixture was reacted at a stirring speed of 1000 r / min for 3 min. The mixture was filled in a fixed mold at a pressure of 0.4 kg / cm 2 The micro-foaming was performed for 150 minutes, and the carbon-based composite shaped filter material was obtained after demoulding.
[0063] The test results show that the porosity of the carbon-based composite filter material is 34.55% and the pore volume is 3.39*10 6 mm 3 The diameter of the microfoam structure is 20 to 60 μm.
[0064] Comparative Example 1
[0065] The difference from Example 5 is that equal amounts of amine antioxidants, phenolic antioxidants and anti-wear additives are directly added to the engine oil without modifying the carbon material.
[0066] Comparative Example 2
[0067] The difference from Example 5 is that the carbon-based material used has not been functionalized with amine antioxidants, phenolic antioxidants and anti-wear additives, and the polyurethane component A used is a single component polyether polyol, which has not been compounded or added with additives. After testing, the porosity of the carbon-based composite shaped filter material is 25.07%, and the pore volume is 1.89*10 6 mm 3 .
[0068] Comparative Example 3
[0069] Use commercial paper filters.
[0070] The carbon-based composite shaped filter materials of Examples 1-5 and Comparative Examples 1-2 were packaged to obtain a carbon-based composite filter, which was loaded into a vehicle with the same model of commercial paper filter in Comparative Example 3 for actual vehicle testing. After the actual vehicle traveled 10,000 km, the relevant indicators of the engine oil were tested. The moisture content was determined according to ASTM D6304-20, the kinematic viscosity was determined according to ASTM D445-21el, the viscosity index was determined according to ASTM D2270-10, the acid value was determined according to ASTM D664-18e2, the gasoline dilution was determined according to ASTM D3525-20, the oxidation value and nitration value were determined according to ASTM E2412-10 differential spectrum method, and the iron, copper and silicon content were determined according to ASTM D5185-18. The test results are shown in Table 1 below:
[0071] Table 1 Test results of oil-related indicators after 10,000 km of actual vehicle operation
[0072]
[0073] It can be seen from the data in Table 1 that, compared with Comparative Examples 1-3, Examples 1-5 of the present invention have less increase in moisture content, less kinematic viscosity decay, less viscosity index decay, less acid value increase, lower gasoline dilution, lower oxidation value and nitration value, and lower iron, copper and silicon content after 10,000 km of use, indicating that the engine oil has good quality, delayed decay and failure, and extended the service life of the engine oil.
[0074] Figure 1 In the figure, (a) is a diagram showing the body structure of a carbon-based composite shaped filter material, and (b) is a diagram showing the micro-foam structure formed between carbon material particles by inserting and micro-foaming a carbon material compounded with a two-component polyurethane.
[0075] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a carbon-based composite shaped filter material for extending the service life of engine oil, characterized in that: Functional compounds are used to perform functional modification on carbon materials to obtain functionalized carbon materials; then, the carbon-based composite shaped filter material is prepared by inserting micro-foaming and composite shaping with polyurethane; the functional compound is composed of amine antioxidants, phenolic antioxidants and anti-wear additives; and the carbon-based composite shaped filter material has a micro-foam structure.
2. The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil according to claim 1, characterized in that: The three types of functional compounds are respectively composite-enriched and modified with carbon materials to obtain amine antioxidant modified carbon materials, phenol antioxidant modified carbon materials and anti-wear modified carbon materials; the functionalized carbon material is prepared by mixing amine antioxidant modified carbon materials, phenol antioxidant modified carbon materials and anti-wear modified carbon materials, and the proportions are 20% to 30%, 50% to 60%, and 10% to 30%, respectively, and the sum of the weight percentages of the three types of modified carbon materials is 100%.
3. The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil according to claim 2, characterized in that: The content of amine antioxidant in the amine antioxidant modified carbon material is 1% to 3%, the content of phenol antioxidant in the phenol antioxidant modified carbon material is 1% to 5%, and the content of anti-wear additive in the anti-wear modified carbon material is 1% to 5%.
4. The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil according to claim 1, characterized in that: The amine antioxidant is one of N,N'-dimethyl-p-phenylenediamine or N,N'-diphenyl-p-phenylenediamine or a mixture of two thereof; the phenol antioxidant is one of 2,6-di-tert-butylphenol or 2,6-di-tert-butyl-4-methylphenol or a mixture of two thereof; and the anti-wear additive is one of tricresyl phosphate or a mixture of two thereof.
5. The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil according to claim 1, characterized in that: The mass ratio of the functionalized carbon material to the polyurethane is 2:1 to 8:
1.
6. The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil according to claim 1, characterized in that: The polyurethane comprises component A and component B. Component A is obtained by compounding polyether polyol, polyester polyol and an auxiliary agent. Component B is diphenylmethane diisocyanate. The auxiliary agent is one of organic tin or triethanolamine or a mixture of the two.
7. The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil according to claim 6, characterized in that: The preparation process is insert micro-foaming composite shaping, and the specific steps are: at room temperature, add polyurethane component A to the functionalized carbon material and mix evenly; then add polyurethane component B, stir and react quickly, the stirring speed is 300-1500r / min, and the time is 1-10min; then fill it into a fixed mold and perform micro-foaming molding at room temperature under controlled pressure, and the pressure is 0.1-1kg / cm 2 , time is 10 to 240 minutes.
8. The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil according to claim 6, characterized in that: The following steps are involved: (1) An amine antioxidant is dissolved in ethanol to prepare a solution, and then ultrasonically impregnated with a carbon material, filtered, and vacuum dried to obtain an amine antioxidant modified carbon material; a phenolic antioxidant is dissolved in ethanol to prepare a solution, and then ultrasonically impregnated with a carbon material, filtered, and vacuum dried to obtain a phenolic antioxidant modified carbon material; an anti-wear modifier is dissolved in ethanol to prepare a solution, and then ultrasonically impregnated with a carbon material, filtered, and vacuum dried to obtain an anti-wear modified carbon material; (2) Amine antioxidant modified carbon material, phenol antioxidant modified carbon material and anti-wear modified carbon material are mixed to obtain a functionalized carbon material; (3) The polyurethane comprises A and B, polyester polyol and an auxiliary agent are added to the polyether polyol to obtain the polyurethane component A, wherein the auxiliary agent is organic tin or triethanolamine; (4) adding the polyurethane component A obtained in step (3) to the functionalized carbon material after compounding in step (2), uniformly mixing at room temperature, then adding the polyurethane component B for rapid stirring and reaction, filling the mixture into a fixed mold for pressure-controlled micro-foaming at room temperature, and obtaining a carbon-based composite shaped filter material after demolding; the component B is diphenylmethane diisocyanate.
9. The method for preparing the carbon-based composite shaped filter material for extending the service life of engine oil according to claim 6, characterized in that: The mass ratio of polyether polyol, polyester polyol and auxiliary agent is (2-5):1:(0.05-0.5); the mass ratio of component A to component B is 0.5:1-3: