Cleaning solution for residues after etching of semi-water-based chip as well as preparation method and application of cleaning solution
After dry etching, the problem of air bubbles and corrosion on the residue cleaning of the residue cleaning solution after dry etching is solved, and the problem of air bubbles and corrosion on the aluminum is easily generated by dry etching is achieved. Efficient, fast and thorough cleaning results reduce product defects and costs.
Patent Information
- Application Number
- CN202411040308.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-26
AI Technical Summary
After dry etching, the residue cleaning liquid is prone to bubbles, which makes the substrate difficult to thoroughly clean and has obvious corrosion problems on aluminum metal.
Using a semi-water-based chip etching residue cleaning solution, including a composite functional agent consisting of neochlorogenic acid and cysium esters, it has the dual functions of corrosion inhibition and emulsification stability, and the esterification reaction is used to generate esteresis to improve cleaning. Efficiency and pure immersion cleaning without ultrasonic process.
It realizes efficient, rapid and thorough cleaning of the residue after etching, reduces product defects and production costs, improves product reliability, and significantly reduces the corrosion rate of aluminum.
Smart Images

Figure CN119020113A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor manufacturing technology, and in particular relates to a semi-aqueous chip post-etching residue cleaning liquid and a preparation method and application thereof. Background Art
[0002] In the integrated circuit manufacturing process, cleaning of particles, metal pollution, oxide film and by-products generated in the production process on the wafer surface is one of the most commonly used process steps. The cleaning effect seriously affects the performance of the integrated circuit and the quality and reliability of the device.
[0003] With the different requirements for integrated circuit performance at different development stages, the cleaning technology in the existing integrated circuit manufacturing process is also constantly being updated. Commonly used wafer cleaning technologies include wet cleaning and dry cleaning. Wet cleaning generally uses highly corrosive and oxidizing inorganic chemical solvents to cause impurity particles on the surface of the wafer to react chemically with the solvent to generate gas or be dissolved and separated from the wafer surface. Dry cleaning refers to the cleaning process without the use of chemical solvents, such as gas phase dry cleaning technology and beam cleaning technology. Due to the high cost of dry cleaning technology, it has always restricted its large-scale promotion and development; wet cleaning technology still occupies a dominant position in the cleaning process of semiconductor factories due to its simplicity and high efficiency.
[0004] In order to solve the problem of cross contamination of wafers, the wafer cleaning method has evolved from multi-tank immersion cleaning in mass production to single wafer cleaning. In the wet cleaning process, various factors such as the environment, production equipment and process deviations will cause various defects in the wafer during production, such as various particles on the wafer surface, etching residues, organic residues, water marks and metal wire corrosion, etc. These defects will affect the realization of device performance to varying degrees.
[0005] Among them, aluminum metal corrosion is a fatal defect that not only seriously affects the yield and reliability of the chip, but also affects the yield of the integrated circuit manufacturing production line. The photoresist cleaning solution for the aluminum process integrated circuit is mainly composed of alkaline organic compounds. For the aluminum process of integrated circuits, since metal aluminum is an amphoteric metal element, the general cleaning solution has more stringent cleaning conditions. For example, when the cleaning time is long and the cleaning temperature is high, it is easy to cause corrosion of the aluminum wire in an alkaline environment, resulting in the damage of the integrated circuit.
[0006] As the size of integrated circuit manufacturing technology shrinks, the cleaning requirements for photoresist films and residues after ashing become more stringent, so the cleaning fluid is required to have higher wetting ability. Dry etching cleaning fluid generally adds surfactants to reduce the surface tension between the residues after dry etching and the substrate, but its bubbling nature will cause the dry etching cleaning fluid to produce foam, making it difficult to thoroughly clean the substrate.
[0007] Therefore, it is necessary not only to improve the balance of surface tension, but also to improve the stripping performance of residues, so that the stripping of residues can be more complete, faster and more thorough. Summary of the invention
[0008] The technical problem solved by the invention is that the residual cleaning liquid after dry etching has many bubbles and is difficult to clean, and has obvious corrosion to Al.
[0009] In view of the technical problems existing in the prior art, the present invention proposes a semi-aqueous cleaning solution for chip post-etching residues and its preparation method and use. The cleaning solution is highly efficient and has a strong cleaning ability for Al-line process post-etching residues. It can maintain extremely excellent cleaning efficiency only under pure immersion process conditions without ultrasonic process and cleaning, thereby reducing product defects, improving product reliability, and reducing production costs.
[0010] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising" and similar meanings, and closed-ended "consisting of..." and similar meanings.
[0011] In order to solve the above-mentioned technical problems, the present invention adopts the following solutions:
[0012] A semi-aqueous chip post-etching residue cleaning solution, characterized in that it comprises the following components, calculated by weight:
[0013]
[0014]
[0015] Wherein, the composite functional agent is prepared from neochlorogenic acid and lithospermic acid.
[0016] Furthermore, the mass ratio of the neochlorogenic acid to lithospermic acid is 1:10.
[0017] Furthermore, the preparation method of the composite functional agent comprises the following steps:
[0018] Step 1: First add neochlorogenic acid and lithospermic acid into the test tube, then add concentrated sulfuric acid, then fix and heat at the bottom of the test tube with an alcohol lamp;
[0019] Step 2: First use the inner flame of an alcohol lamp to heat slightly for 2-4 minutes, then use the outer flame of an alcohol lamp to heat for 10-15 minutes to evaporate the generated esterification;
[0020] Step 3: Collect the generated ester, wash and dry it to obtain the composite functional agent.
[0021] Furthermore, the mass fraction of concentrated sulfuric acid in step 1 is 3 times that of neochlorogenic acid.
[0022] Furthermore, in the step 1, neochlorogenic acid and lithospermic acid are respectively prepared into 50% aqueous solutions, and then added into a test tube for reaction.
[0023] Furthermore, the pH adjuster is one or more of malic acid, citric acid and tartaric acid.
[0024] Furthermore, the organic solvent is one or more of N,N-dimethylacetamide, 1,1-cyclohexyldiacetic acid monoamide, 2-hydroxyisobutyramide, and p-aminobenzamide.
[0025] Furthermore, the protective agent is one or more of polyethylene glycol 200, polyethylene glycol 400, and polyethylene glycol 600.
[0026] The present invention also discloses a method for preparing a semi-aqueous chip post-etching residue cleaning solution, which is characterized by comprising the following steps:
[0027] Step 1: Weigh each component according to the proportion;
[0028] Step 2: Add all components except ultrapure water and composite functional agent into a container and stir until all materials are completely dissolved. Add 1 / 2 amount of composite functional agent and all ultrapure water while stirring, continue stirring for 2-5 minutes, then add the remaining composite functional agent and stir until all materials are completely dissolved to obtain the semi-aqueous chip post-etching residue cleaning solution.
[0029] The present invention also discloses a method for cleaning residues after etching of a semi-aqueous chip using a cleaning solution, which is characterized by comprising the following steps:
[0030] Step 1: The prepared semi-aqueous chip post-etching residue cleaning solution is prepared with ultrapure water to form an aqueous solution with a mass percentage concentration of 15%-35%;
[0031] Step 2: Soak the semiconductor chip in the aqueous solution prepared in step 1 at 30-50° C. for 7-15 minutes to obtain a soaked semiconductor chip;
[0032] Step 3: Rinse the soaked semiconductor chip in anhydrous ethanol for at least two times, then rinse it with ultrapure water and blow dry it with nitrogen, thus completing the cleaning of the semiconductor chip.
[0033] The invention also discloses the use of a semi-aqueous cleaning solution for cleaning residues after chip etching in cleaning semiconductor chips.
[0034] In the present invention, in order to further optimize the effect of the cleaning solution, its various components can be further optimized: 0.2-0.4 parts of composite functional agent; 2.5-3.5 parts of pH regulator; 0.2-0.7 parts of protective agent; 0.3-0.8 parts of hydrofluoric acid; 0.5-1 parts of ammonium fluoride; 45-55 parts of organic solvent; 25-35 parts of ultrapure water.
[0035] In the preparation method of the composite functional agent of the present invention, the purpose of slight heating over low heat is to prevent the unreacted lithospermic acid and neochlorogenic acid from being evaporated, and the purpose of evaporating over high heat in the later stage is to separate the esters from the reaction system, which is beneficial for the reversible reaction equilibrium to move toward the direction of ester formation.
[0036] In step 2 of preparing the composite functional agent of the present invention, the ester is completely evaporated when the liquid level in the receiving bottle no longer fluctuates.
[0037] In the present invention, the organic solvent is preferably N,N-dimethylacetamide.
[0038] In the present invention, the structural formula of the new chlorogenic acid is as follows:
[0039]
[0040] In the present invention, the structural formula of lithospermic acid is as follows:
[0041]
[0042] The inventors have found that neochlorogenic acid and lithospermic acid contain more activated hydroxyl groups and carboxyl groups. The two hydroxyl groups and one carboxyl end in the structure of neochlorogenic acid can be connected to the carboxyl end and hydroxyl group of lithospermic acid, respectively, and an esterification reaction occurs under the catalysis of concentrated sulfuric acid to form an ester. The ester is a substance with a head-to-tail structure, and a capsule-like structure is formed inside the two macromolecules, forming adsorption within the system, which can effectively remove surface residues.
[0043] In the present invention, the composite functional agent has the dual functions of corrosion inhibition and emulsification stabilization. Its corrosion inhibition function can protect the chip from corrosion, while its emulsification stabilization function has excellent emulsification performance and stability in the system, thereby ensuring uniform mixing of oil and water in the entire system.
[0044] The composite functional agent of the present invention, hydrogen fluoride and ammonium fluoride can jointly enhance the cleaning ability of the cleaning liquid for polymers, and can also play a role in protecting and resisting corrosion on the substrate from the side.
[0045] The present invention provides a semi-aqueous chip post-etching residue cleaning solution and a preparation method and use thereof, which have the following beneficial effects:
[0046] 1. The composite functional agent of the present invention is a new chlorogenic acid and lithospermum ester, which can thoroughly clean the wax layer, grinding dirt and other pollutants attached to the chip, and will not form wax on the surface of the solution, nor will it cause dirt to stick back to the chip; the composite functional agent has the dual functions of corrosion inhibition and emulsification stabilization. Its corrosion inhibition function can protect the chip from corrosion, and its emulsification stabilization function has excellent emulsification performance and stability performance in the system, thereby ensuring uniform mixing of oil and water in the entire system.
[0047] 2. The composite functional agent of the present invention, together with hydrogen fluoride and ammonium fluoride, enhances the cleaning ability of the cleaning solution for polymers, and can also protect and resist corrosion of the substrate from the side.
[0048] 3. The cleaning solution of the present invention has excellent cleaning performance, can achieve excellent cleaning effect, and has no corrosion to the chip.
[0049] 4. The cleaning solution of the present invention has low volatile loss. After cleaning, the chip does not need to be rinsed with acetone, but only needs to be rinsed with anhydrous ethanol or pure water, which is harmless to the environment and human body. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 : Infrared spectrum of the synthesized composite functional agent;
[0051] Figure 2 : Microscope picture of the chip before cleaning, magnified 8000 times;
[0052] Figure 3 : A microscope picture of a chip after being cleaned using the cleaning solution prepared in Comparative Example 1, magnified 4000 times;
[0053] Figure 4 : This is a microscope picture magnified 8000 times of the chip after cleaning with the cleaning solution prepared in Example 1. DETAILED DESCRIPTION
[0054] The present invention will be further described below in conjunction with specific embodiments and accompanying drawings:
[0055] Table 1 Examples 1-6
[0056]
[0057]
[0058] Table 2 Comparative Examples 1-2
[0059]
[0060] Table 3 Test data
[0061]
[0062] The preparation method of the composite functional agent in the embodiment of the present invention:
[0063] Place neochlorogenic acid, lithospermic acid and concentrated sulfuric acid in a dry 50 mL test tube, mix well and add 2 zeolites.
[0064] The mass ratio of neochlorogenic acid, concentrated sulfuric acid and lithospermic acid is 1:3:10. Neochlorogenic acid and lithospermic acid are prepared into 50% aqueous solutions respectively, and then added into the test tube for reaction.
[0065] Install the water separator and reflux condenser, add water to the side pipe in the water separator, then drain some of the water, that is, the water surface is 3mm away from the side pipe, and mark the water layer interface.
[0066] Heat to reflux, first use the inner flame of an alcohol lamp to heat slightly for 3 minutes, then use the outer flame of an alcohol lamp to heat for 13 minutes to evaporate the generated ester.
[0067] Note the time when the first drop of reflux liquid falls, and control the droplet flow rate in the condenser to 1-2d / s.
[0068] When the water layer interface in the water separator no longer rises, it means that the reaction is basically completed and the reflux is stopped.
[0069] After cooling, remove the reflux condenser and pour the ester layer in the water separator and the reaction solution in the test tube into the separatory funnel.
[0070] Add appropriate amount of ultrapure water to the separatory funnel for washing and remove the water layer; wash the ester layer again with 10 mL of water and remove the water layer; pour the ester layer material into a small conical flask to dry and set aside.
[0071] In the embodiments and comparative examples of the present invention, multiple groups of cleaning liquid products were prepared, and the preparation methods thereof are as follows:
[0072] Step 1: Weigh each component according to the proportion;
[0073] Step 2: Add all components except ultrapure water and composite functional agent into a container and stir until all materials are completely dissolved. Add 1 / 2 amount of composite functional agent and all ultrapure water while stirring, continue stirring for 3 minutes, then add the remaining composite functional agent and stir until all materials are completely dissolved to obtain the semi-aqueous chip post-etching residue cleaning solution.
[0074] About performance testing and description:
[0075] Performance 1 The test method for cleaning effect is:
[0076] Step 1: Prepare the prepared chip cleaning solution with ultrapure water to an aqueous solution with a mass percentage concentration of 20%;
[0077] Step 2: Soak the Al chip in the aqueous solution prepared in step 1 at 35° C. for 10 min to obtain the soaked Al chip;
[0078] Step 3: Rinse the soaked semiconductor chip twice in anhydrous ethanol, then rinse it with ultrapure water and blow dry it with nitrogen, thus completing the cleaning of the semiconductor chip.
[0079] Performance 2 The test method for metal corrosion is:
[0080] The four-probe method is used to test the corrosion performance of different cleaning solutions on metals. The specific test method is as follows:
[0081] A 2cm×2cm wafer was tested for initial film thickness Th0 before immersion using a four-probe tester.
[0082] Each time the four-probe test is performed, the environment of the instrument must be kept consistent. Then the wafer is immersed in a 35°C cleaning solution for 10 minutes. The wafer is then taken out and immediately rinsed with ultrapure water and anhydrous ethanol. After each rinse, nitrogen is used to blow dry the wafer to keep it clean. After the wafer is clean, the four-probe tester is used again to test the wafer that has just been cleaned to obtain the film thickness. The corrosion rate is calculated based on the change in film thickness before and after the two times. Calculation.
[0083] Analysis of the test results:
[0084] It can be seen from the data in Table 3 that the corrosion rate of Al is greatly reduced for the chip cleaned with the cleaning solution prepared in the embodiment of the present invention, which plays an excellent protective role for metal Al.
[0085] In comparative example 1, due to the lack of the composite functional agent, the F ions in the cleaning solution will directly contact with the aluminum, resulting in an increase in the corrosion rate of the aluminum and the appearance of through holes. After the composite functional agent is added, the F ions in the solution will be indirectly isolated from direct contact with the aluminum, greatly reducing the corrosion of the cleaning solution to Al. For polymer cleaning, the composite functional agent itself has a capsule-like structure, which can wrap the polymer in the form of a package to take away the residue, thereby achieving the cleaning effect.
[0086] In comparative example 2, due to the lack of protective agent, the F ions in the cleaning solution will corrode Al to a certain extent, increasing the corrosion rate of aluminum. After adding the protective agent, it covers the metal through its specific configuration, preventing the F ions from directly contacting the aluminum, thereby reducing the occurrence of corrosion; the protective agent can also further reduce aluminum corrosion by affecting the activity of metal ions and the chemical balance of the solution.
[0087] Further comparison is made through the attached drawings in the specification:
[0088] Figure 1 This is the infrared spectrum of the synthesized composite functional agent.
[0089] from Figure 1 It can be seen that at 1750cm -1 The absorption peak that appears is the ester group, indicating that the composite functional agent has been esterified to generate the target substance.
[0090] Figure 2 This is a microscope picture of the chip before cleaning, magnified 8000 times; Figure 3 This is a microscope picture of a chip after being cleaned using the cleaning solution prepared in Comparative Example 1, magnified 4000 times; Figure 4 This is a microscope picture of the chip after being cleaned with the cleaning solution prepared in Example 1, magnified 8000 times.
[0091] from Figure 2-Figure 4 From the comparison, it can be seen that after cleaning with the cleaning solution prepared in Comparative Example 1, through holes appear on the surface of the chip, indicating poor protection of the substrate, while after cleaning with the cleaning solution prepared in Example 1, the surface of the chip is clean without residue and is basically corrosion-free.
[0092] The composite functional agent of the present invention can thoroughly clean the wax layer, grinding dirt and other pollutants attached to the chip, and will not form wax on the surface of the solution, nor will it cause dirt to stick back to the chip. The composite functional agent of the present invention has the dual functions of corrosion inhibition and emulsification stabilization. The corrosion inhibition function can protect the chip from corrosion, and the emulsification stabilization function has excellent emulsification performance and stability performance in the system, thereby ensuring the uniform mixing of oil and water in the entire system. The cleaning liquid of the present invention has low volatile loss. After cleaning, the chip does not need to be rinsed with acetone, but only needs to be rinsed with anhydrous ethanol and pure water, which is harmless to the environment and human body.
[0093] The present invention is described exemplarily above in conjunction with the embodiments and drawings. It is obvious that the implementation of the present invention is not limited to the above-mentioned methods. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A semi-aqueous chip etching residue cleaning solution, characterized in that: Calculated by weight, it includes the following components: Wherein, the composite functional agent is prepared from neochlorogenic acid and lithospermic acid.
2. The semi-aqueous chip post-etching residue cleaning solution according to claim 1, characterized in that: The preparation method of the composite functional agent comprises the following steps: Step 1: First add neochlorogenic acid and lithospermic acid into the test tube, then add concentrated sulfuric acid, then fix and heat at the bottom of the test tube with an alcohol lamp; Step 2: First use the inner flame of an alcohol lamp to heat slightly for 2-4 minutes, then use the outer flame of an alcohol lamp to heat for 10-15 minutes to evaporate the generated esterification; Step 3: Collect the generated ester, wash and dry it to obtain the composite functional agent.
3. The semi-aqueous chip post-etching residue cleaning solution according to claim 2, characterized in that: The mass ratio of the neochlorogenic acid to lithospermic acid in step 1 is 1:
10.
4. The semi-aqueous chip post-etching residue cleaning solution according to claim 2, characterized in that: In the step 1, neochlorogenic acid and lithospermic acid are respectively prepared into 50% aqueous solutions, and then added into a test tube for reaction.
5. The semi-aqueous chip post-etching residue cleaning solution according to claim 1, characterized in that: The pH regulator is one or more of malic acid, citric acid and tartaric acid.
6. The semi-aqueous chip post-etching residue cleaning solution according to claim 1, characterized in that: The organic solvent is one or more of N,N-dimethylacetamide, 1,1-cyclohexyldiacetic acid monoamide, 2-hydroxyisobutyramide and p-aminobenzamide.
7. The semi-aqueous chip post-etching residue cleaning solution according to claim 1, characterized in that: The protective agent is one or more of polyethylene glycol 200, polyethylene glycol 400 and polyethylene glycol 600.
8. A method for preparing a semi-aqueous chip post-etching residue cleaning solution according to any one of claims 1 to 7, characterized in that The following steps are included: Step 1: Weigh each component according to the proportion; Step 2: Add all components except ultrapure water and composite functional agent into a container and stir until all materials are completely dissolved. Add 1 / 2 amount of composite functional agent and all ultrapure water while stirring, continue stirring for 2-5 minutes, then add the remaining composite functional agent and stir until all materials are completely dissolved to obtain the semi-aqueous chip post-etching residue cleaning solution.
9. A method for cleaning the residue after etching of a semi-aqueous chip according to any one of claims 1 to 7, characterized in that The steps include: Step 1: The prepared semi-aqueous chip post-etching residue cleaning solution is prepared with ultrapure water to form an aqueous solution with a mass percentage concentration of 15%-35%; Step 2: Soak the semiconductor chip in the aqueous solution prepared in step 1 at 30-50° C. for 7-15 minutes to obtain a soaked semiconductor chip; Step 3: Rinse the soaked semiconductor chip in anhydrous ethanol for at least two times, then rinse it with ultrapure water and blow dry it with nitrogen, thus completing the cleaning of the semiconductor chip.
10. Use of the semi-aqueous chip post-etching residue cleaning solution according to any one of claims 1 to 7 in cleaning semiconductor chips.