Smelting method for controlling nitrogen content of low-carbon high-chromium steel

Through the KR-BOF-RH-LF-CC process path, combined with deep desulfurization, oxygen blowing decarbonization and full protection casting, the problem of nitrogen content control in the smelting of low-carbon high-chromium steel is solved, and low-nitrogen finished products are achieved and improved Product performance and process stability.

CN119020553APending Publication Date: 2024-11-26TANGSHAN IRON & STEEL GROUP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411240702.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-27
Filing Date
2024-09-05
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing smelting process is difficult to effectively control the nitrogen content in low-carbon and high-chromium steel, resulting in a high nitrogen content of the finished product, affecting the toughness and molding performance of the steel.

Method used

Using the KR-BOF-RH-LF-CC process path, the KR desulfurization, BOF smelting, RH refining, LF refining and continuous casting process include deep desulfurization, oxygen blowing decarbonization, micro-positive pressure operation in the furnace, low carbon Ferrochromium is added in batches, calcium line feeding and full protection casting, and each process parameter is controlled to reduce nitrogen content.

Benefits of technology

It effectively reduces the finished nitrogen content of low-carbon and high-chromium steel to ≤66ppm, and improves the molding performance and process stability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020553A_ABST
    Figure CN119020553A_ABST
Patent Text Reader

Abstract

The invention discloses a smelting method for controlling the nitrogen content of low-carbon high-chromium steel. The smelting method comprises the processes of KR desulfurization, BOF smelting, RH refining, LF refining and continuous casting. According to the KR desulfurization process, a deep desulfurization mode is adopted, and the outbound S content is smaller than or equal to 0.0015%; in the BOF smelting process, the C content of molten iron entering a furnace is larger than or equal to 4.5%, the scrap steel ratio is smaller than or equal to 10%, and argon is blown from the bottom in the whole process In the RH refining process, oxygen blowing decarburization is conducted, the decarburization time is 16-18 min, and the end target carbon content is smaller than or equal to 15 ppm; after decarburization is completed, 500-100 Nm < 3 > oxygen is reblown to heat the molten steel; the total oxygen content in RH outbound steel is 150-300 ppm, and the total iron content in slag is 8-12%; in the LF refining process, in-furnace micro-positive pressure operation is adopted for LF refining, and the thickness of slag ranges from 80 mm to 100 mm. The nitrogen content of the low-carbon high-chromium steel finished product is smaller than or equal to 66 ppm, and the problem that nitrogen is increased seriously in the low-carbon steel alloy steel smelting process is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, in particular to a smelting method for controlling nitrogen content in low-carbon high-chromium steel. Background Art

[0002] High nitrogen content in steel can easily cause pores in continuous casting billets. In addition, nitrogen can easily react with Ti, V, etc. to form brittle nitrides. Nitrides in the heat affected zone (HAZ) of welding decompose, resulting in an increase in free nitrogen content. The increase in nitrogen content causes the low-temperature brittle transition temperature of carbon microalloy steel to rise and the toughness to deteriorate. During the steelmaking process, nitrogen should be controlled at a low level as much as possible.

[0003] Low-carbon high-alloy steels, such as weathering steel Q350EW, cannot meet the low-carbon requirements under high-alloy conditions using the conventional KR-BOF-LF-RH-CC steelmaking process. It is necessary to change the idea and adopt the KR-BOF-RH-LF-CC steelmaking process. The converter is oxygen-free and no alloying treatment is performed. The RH refining uses an ultra-low carbon mode to remove carbon from the steel to an extremely low level, and then alloys are added to meet the low-carbon requirements of the steel. However, the biggest drawback of KR-BOF-RH-LF-CC is that the converter does not perform alloying, and the RH process is moved forward and vacuum degassing cannot be performed, resulting in a high nitrogen content in the finished product. In addition, the addition of a large amount of alloys during the LF refining process causes serious nitrogen increase in the alloy. For example, the nitrogen content in the alloy low-carbon ferrochrome is 0.025% to 0.030%, and the theoretical nitrogen increase is about 22 to 26 ppm when the Cr content of the finished product is 4.5%. The addition of a large amount of alloys during the refining process causes a long smelting cycle, and the temperature drop during the refining process is serious, requiring a long time to heat up with electricity. These factors all cause serious nitrogen increase in the refining process. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a smelting method for controlling the nitrogen content of low-carbon high-chromium steel to ensure the nitrogen content of the finished product.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: it includes KR desulfurization, BOF smelting, RH refining, LF refining and continuous casting process; the process of each process is: The KR desulfurization process: adopts deep desulfurization mode, and the outgoing S content is ≤0.0015%; The BOF smelting process: the C content of the molten iron entering the furnace is ≥4.5%, the scrap ratio is ≤10%, and argon is blown at the bottom throughout the process; The RH refining process: oxygen blowing decarburization, the target carbon content after decarburization is ≤15ppm; after decarburization is completed, 500-100Nm 3 Oxygen heats up the molten steel; the total oxygen content in the RH steel is 150-300ppm, and the total iron content in the slag is 8-12%; The LF refining process: LF refining adopts a slightly positive pressure operation in the furnace, the slag thickness is 80-100mm, low carbon ferrochrome is added according to the target composition, the low carbon ferrochrome is added in batches, the temperature is raised once every 5-6t of low carbon ferrochrome is added, the alloying target temperature is 1580-1600°C, the bottom blowing flow rate is 500-600NL / min; after the refining is completed, the calcium wire is fed, and the feeding wire speed is 160-180m / min; The continuous casting process includes full protection casting and the residual oxygen content in the tundish is ≤0.50%.

[0006] Furthermore, in the BOF smelting process, the final oxygen level is controlled at 500-700 ppm, the final temperature is 1650-1670° C., high calcium lime and fluorite are added during the steelmaking process, and deoxidation and alloying are not performed.

[0007] Furthermore, the RH refining process: pure circulation after decarburization ≥ 6 minutes, minimum vacuum ≤ 2 mbar, RH outlet temperature 1570-1580°C.

[0008] Furthermore, in the LF refining process, aluminum blocks and aluminum wires are added during the last composition adjustment, the soft blowing flow rate is 20-80NL / min and no molten steel is exposed, the LF smelting cycle is 100-120min, the power supply time is ≤50min, and the LF outlet temperature is 1570-1580°C.

[0009] Furthermore, in the continuous casting process, a carbon-free tundish covering agent is used, and the tundish slag thickness is 40 to 60 mm.

[0010] The beneficial effects of the above technical scheme are as follows: the present invention is based on the KR-BOF-RH -LF-CC process path, the desulfurization task is moved forward to the KR desulfurization process, the S content is ≤0.0015% to reduce the burden of LF refining, and the LF refining desulfurization task is liberated after the KR deep desulfurization treatment, and the molten steel oxidation in the RH and LF refining processes is improved, which is convenient for the formulation of nitrogen control measures in the subsequent links. The converter adopts measures such as low scrap steel ratio, clear carbon content of molten iron entering the furnace, and argon blowing throughout the process to increase the carbon oxygen reaction and stirring intensity in the steel to remove the nitrogen content in the steel, thereby effectively controlling the nitrogen content in the converter link. RH refining adopts oxygen blowing decarburization and heating process to increase the total oxygen content of molten steel and the total iron content in slag, providing conditions for LF refining nitrogen control. LF refining adopts positive pressure in the furnace, ensures submerged arc, optimizes the low-carbon ferrochrome addition method, optimizes the bottom blowing flow rate and calcium wire feeding method, and focuses on controlling the oxidation of molten steel in the LF refining process, especially the addition of aluminum blocks and aluminum wires in the last component adjustment, which effectively reduces the increase of nitrogen in the refining process. The continuous casting adopts full protection casting measures, and the residual oxygen content in the tundish is ≤0.50%, which reduces the nitrogen increase during the continuous casting process.

[0011] The present invention is based on the KR-BOF-RH-LF-CC process path and adopts key nitrogen control means in the steelmaking process. Under the condition that the nitrogen content in the added low-carbon ferrochrome is 0.025-0.030%, a series of nitrogen control measures in the whole process of the steelmaking process are used to achieve a nitrogen content of ≤66ppm in the finished product of the low-carbon high-chromium hot-rolled steel plate. The present invention effectively solves the serious problem of nitrogen increase in the smelting process of low-carbon steel and alloy steel, effectively improves the forming performance of the product, and has the characteristics of stable process and excellent product performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0013] Figure 1 It is a diagram of the residual oxygen content in the tundish during the casting process of the continuous casting step described in the present invention. DETAILED DESCRIPTION

[0014] The smelting method for controlling nitrogen content in low-carbon high-chromium steel adopts the following chemical composition and mass fraction of low-carbon high-chromium steel: C 0.015%~0.040%, Mn 0.30%~0.45%, S≤0.005%, P≤0.018%, Als 0.025%~0.040%, Cu 0.35%~0.45%, Cr 4.30%~5.00%, Ti 0.010%~0.025%, Nb 0.007%~0.015%, Ni0.25%~0.40%, N≤0.0060%, and the rest are Fe and unavoidable impurity elements. The smelting method for controlling nitrogen content in low-carbon high-chromium steel adopts the KR-BOF-RH-LF-CC steelmaking process path, and each process is described as follows: (1) KR desulfurization process: adopt deep desulfurization mode, the outgoing sulfur content is ≤0.0015wt% to reduce the burden of LF refining; the bright surface area of ​​slag after desulfurization is ≥95%.

[0015] (2) BOF smelting process: C content of molten iron entering the furnace is ≥4.5wt%, scrap ratio is ≤10wt%, argon is blown from the bottom throughout the process, and the bottom blowing gas supply intensity is 0.065~0.082Nm 3 / (min.t); the BOF endpoint oxygen level is controlled at 500-700ppm, and the endpoint temperature is 1650-1670℃; high calcium lime and fluorite are added during the steelmaking process, and deoxidation and alloying are not performed.

[0016] (3) RH refining process: Ultra-low carbon mode is used to blow oxygen to decarburize the molten steel. The decarburization time is 16 to 18 minutes. The target carbon content after decarburization is ≤15ppm. After decarburization, 500 to 100 Nm of oxygen is blown. 3Oxygen is used to heat the molten steel, and the pure circulation after decarburization is ≥6 minutes; the minimum vacuum degree during the RH refining process is ≤2mbar; the RH outlet temperature is 1570-1580℃, the total oxygen content in the RH outlet steel is 150-300ppm, and the total iron content in the slag is 8-12%.

[0017] (4) LF refining process: LF refining adopts a slightly positive pressure operation in the furnace, and the slag thickness is 80-100 mm to ensure the arc buried effect during the power supply process, that is, to ensure that the arc length is ≤70 mm; low carbon ferrochrome is added according to the target composition, and the low carbon ferrochrome is added in batches. The temperature is raised once every 5-6 tons of low carbon ferrochrome is added. The 5-6 tons of low carbon ferrochrome is preferably added in two batches; the nitrogen content of the low carbon ferrochrome is 0.025-0.030wt%; the alloying target temperature is 1580-1600℃; the bottom blowing flow rate is 500-600NL / min, so as to avoid excessive bottom blowing flow causing exposed molten steel and increasing the risk of nitrogen increase; aluminum blocks and aluminum wires are added in the last composition adjustment; calcium wire is fed after refining, with a calcium content target of 0.0015~0.0025wt%, a wire feeding speed of 160~180m / min, and a calcium wire feeding angle of 85~90° to the molten steel surface; soft blowing flow of 20~80NL / min to ensure that no molten steel is exposed; LF smelting cycle of 100~120min, power-on time ≤50min, LF outlet temperature of 1570~1580℃.

[0018] (5) Continuous casting (CC) process: ensure that the shroud and its gasket are intact to ensure the argon sealing effect of the shroud; use carbon-free tundish covering agent, the tundish slag thickness is 40-60mm, and the residual oxygen content in the tundish is ≤0.50wt%. Argon flow control and other requirements for each link of protective casting: the shroud argon pipeline is opened, the argon flow rate is 150-200 NL / min, and the back pressure is ≥0.1bar; the argon flow rate at the tundish upper shroud is 3-6NL / min, and the back pressure is ≥0.1bar; the stopper argon flow rate is 2-4NL / min, and the back pressure is ≥0.1bar; the inter-plate argon blowing flow rate is 3-6NL / min, and the back pressure is ≥0.1bar. The change of residual oxygen content in the tundish during the continuous casting process is shown in Figure 1 As can be seen from the figure, the residual oxygen content in the stable casting process is 0.12-0.40%, which is extremely low. Therefore, it can effectively inhibit the nitrogen addition and secondary oxidation of the molten steel by the atmosphere during the casting process.

[0019] (6) By adopting the above method, the nitrogen content of the finished low carbon high chromium steel hot rolled plate can be achieved to be ≤66ppm.

[0020] Example 1: The smelting method for controlling the nitrogen content of low-carbon high-chromium steel is specifically described as follows.

[0021] KR desulfurization process: KR outgoing station S content is 0.0013%, and the slag bright surface area after desulfurization is 97%. BOF smelting process: BOF scrap ratio is 8%; the C content of hot metal entering the furnace is 4.7%, and argon is blown at the bottom throughout the process, and the bottom blowing gas supply intensity is 0.065~0.079NNm 3 / (min.t); BOF end oxygen level 531ppm, end temperature 1662℃, high calcium lime and fluorite added during steelmaking, no deoxidation alloying. RH refining process: decarburization time 18min, decarburization end carbon content 11ppm, after decarburization completed, additional blowing 65Nm 3 Oxygen is used to heat the molten steel, and the pure circulation after decarburization is 7 minutes, with a minimum vacuum of 1.2 mbar; the RH outlet temperature is 1575℃, the total oxygen in the RH outlet steel is 207ppm, and the total iron content in the slag is 10%. LF refining process: the furnace is operated with a slight positive pressure, the slag thickness is 80mm, low-carbon ferrochrome is added in batches, and the temperature is raised once every two batches of low-carbon ferrochrome 5.6t are added, the alloying temperature is 1592~1598℃, the bottom blowing flow rate is 500~575NL / min, and the aluminum block and aluminum wire are added in the last composition adjustment. After the refining is completed, calcium is fed, and the target calcium content of the wire is 0.0021%, the wire feeding speed is 160m / min, the calcium wire feeding angle is 90° with the steel liquid surface, the soft blowing flow rate is 50NL / min, and the steel liquid cannot be exposed, the LF smelting cycle is 107min, the power-on time is 48min, and the LF outlet temperature is 1573℃. Continuous casting process: The long shroud and its gasket of the continuous casting ladle are intact, a carbon-free tundish covering agent is used, the tundish slag thickness is 40-60mm, and the residual oxygen content of the tundish is 0.47%; argon flow control and other requirements for protecting each link of casting: the argon pipeline of the long shroud is opened, the argon flow rate is 160-185NL / min, and the back pressure is ≥0.1bar; the argon flow rate of the tundish upper shroud is 5-6NL / min, and the back pressure is 0.3bar; the stopper flow rate is 3-4NL / min, and the back pressure is 0.3bar; the argon blowing flow rate between the plates is 5-6NL / min, and the back pressure is 0.4bar.

[0022] The chemical composition and mass percentage of the low-carbon high-chromium steel obtained in this embodiment are shown in Table 1, and the chemical composition of the low-carbon ferrochrome used is shown in Table 2.

[0023] Example 2: The smelting method for controlling the nitrogen content of the low-carbon high-chromium steel is specifically described as follows.

[0024] KR desulfurization process: KR outgoing station S content is 0.0015%, and the slag bright surface area after desulfurization is 96%. BOF smelting process: BOF scrap ratio is 9%; the C content of hot metal entering the furnace is 4.5%, and argon is blown at the bottom throughout the process, and the bottom blowing gas supply intensity is 0.068~0.082Nm 3 / (min.t), BOF end oxygen level 500ppm, end temperature 1650℃, high calcium lime and fluorite added during steelmaking, no deoxidation alloying. RH refining process: decarburization time 16min, decarburization end carbon content 15ppm, after decarburization completed, additional blowing 100Nm 3 Oxygen is used to heat the molten steel, and the pure circulation after decarburization is 6 minutes, with a minimum vacuum of 1.5mbar; the RH outlet temperature is 1580℃, the total oxygen in the RH outlet steel is 250ppm, and the total iron content in the slag is 12%. LF refining process: the furnace is operated with a slight positive pressure, the slag thickness is 100mm, low-carbon ferrochrome is added in batches, and the temperature is raised once every two batches of low-carbon ferrochrome 6t are added, the alloying temperature is 1592~1600℃, the bottom blowing flow rate is 565~600NL / min, and aluminum blocks and aluminum wires are added in the last composition adjustment. After the refining is completed, calcium wire is fed, and the calcium content target is 0.0025%, the feeding wire speed is 180m / min, the calcium wire feeding angle is 89° with the steel liquid surface, and the soft blowing flow rate is 45NL / min, and the steel liquid cannot be exposed; the LF smelting cycle is 103min, the power-on time is 46min, and the LF outlet temperature is 1570℃. Continuous casting process: The long shroud and its gasket of the continuous casting ladle are intact, a carbon-free tundish covering agent is used, the tundish slag thickness is 40-55mm, and the residual oxygen content of the tundish is 0.37%; argon flow control and other requirements for protecting each link of casting: the argon pipeline of the long shroud is opened, the argon flow rate is 185-200NL / min, and the back pressure is ≥0.1bar; the argon flow rate at the upper shroud of the tundish is 4-5NL / min and the back pressure is 0.2bar; the stopper flow rate is 3-4NL / min and the back pressure is 0.1bar; the argon blowing flow rate between the plates is 4-5NL / min and the back pressure is 0.4bar.

[0025] The chemical composition and mass percentage of the low-carbon high-chromium steel obtained in this embodiment are shown in Table 1, and the chemical composition of the low-carbon ferrochrome used is shown in Table 2.

[0026] Example 3: The smelting method for controlling the nitrogen content of the low-carbon high-chromium steel is specifically described as follows.

[0027] KR desulfurization process: KR outgoing station S content is 0.0010%, and the slag bright surface area after desulfurization is 97%. BOF smelting process: BOF scrap ratio is 10%; the C content of hot metal entering the furnace is 4.8%, and argon is blown at the bottom throughout the process, and the bottom blowing gas supply intensity is 0.066~0.080Nm 3 / (min.t); BOF end oxygen level 700ppm, end temperature 1670℃, high calcium lime and fluorite added during steel tapping, no deoxidation alloying. RH refining process: decarburization time 18min, decarburization end carbon content 13ppm, after decarburization completed, additional blowing 50Nm 3Oxygen is used to heat the molten steel, and the pure circulation after decarburization is 6 minutes, with a minimum vacuum of 2.0 mbar; the RH outlet temperature is 1570℃, the total oxygen in the RH outlet steel is 150ppm, and the total iron content in the slag is 8%. LF refining process: the furnace is operated with a slight positive pressure, the slag thickness is 90mm, low-carbon ferrochrome is added in batches, and the temperature is raised once every two batches of low-carbon ferrochrome 5t are added, the alloying temperature is 1580~1588℃, and the bottom blowing flow rate is 500~570NL / min; aluminum blocks and aluminum wires are added in the last composition adjustment, and calcium wire is fed after refining. The calcium content target is 0.0015%, the feeding speed is 170m / min, the calcium wire feeding angle is 85° with the steel liquid surface, and the soft blowing flow rate is 20NL / min, and the steel liquid cannot be exposed; the LF smelting cycle is 100min, the power-on time is 48min, and the LF outlet temperature is 1580℃. Continuous casting process: The long shroud and its gasket of the continuous casting ladle are intact, a carbon-free tundish covering agent is used, the tundish slag thickness is 45-60mm, and the residual oxygen content of the tundish is 0.35%; argon flow control and other requirements for protecting each link of casting: the argon pipeline of the long shroud is opened, the argon flow rate is 150-175NL / min, and the back pressure is ≥0.2bar; the argon flow rate of the tundish upper shroud is 3-4NL / min, and the back pressure is 0.1bar; the stopper flow rate is 2-3NL / min, and the back pressure is 0.2bar; the argon blowing flow rate between the plates is 3-4NL / min, and the back pressure is 0.2bar.

[0028] The chemical composition and mass percentage of the low-carbon high-chromium steel obtained in this embodiment are shown in Table 1, and the chemical composition of the low-carbon ferrochrome used is shown in Table 2.

[0029] Example 4: The smelting method for controlling the nitrogen content of the low-carbon high-chromium steel is specifically described as follows.

[0030] KR desulfurization process: KR outgoing station S content is 0.0013%, and the slag bright surface area after desulfurization is 95%. BOF smelting process: BOF scrap ratio is 9%, the C content of hot metal entering the furnace is 4.6%, and argon is blown at the bottom of the whole process, and the bottom blowing gas supply intensity is 0.071~0.082Nm 3 / (min.t); BOF end oxygen level 597ppm, end temperature 1661℃, high calcium lime and fluorite added during steel tapping, no deoxidation alloying. RH refining process: decarburization time 17min, decarburization end carbon content 11ppm, after decarburization completed, additional blowing 73Nm 3Oxygen is used to heat the molten steel, and the pure circulation after decarburization is 7 minutes, with a minimum vacuum of 1.8 mbar; the RH outlet temperature is 1573℃, the total oxygen in the RH outlet steel is 178ppm, and the total iron content in the slag is 9%. LF refining process: the furnace is operated with a slight positive pressure, the slag thickness is 80mm, low-carbon ferrochrome is added in batches, and the temperature is raised once every two batches of low-carbon ferrochrome 5.2t are added, the alloying temperature is 1583~1593℃, and the bottom blowing flow rate is 560~600NL / min; aluminum blocks and aluminum wires are added in the last composition adjustment, and calcium is fed after the refining is completed. The calcium content of the wire is 0.0022%, the wire feeding speed is 180m / min, the calcium wire feeding angle is 90° with the steel liquid surface, and the soft blowing flow rate is 80NL / min so that the steel liquid cannot be exposed; the LF smelting cycle is 120min, the power-on time is 50min, and the LF outlet temperature is 1578℃. Continuous casting process: The long shroud and its gasket of the continuous casting ladle are intact, a carbon-free tundish covering agent is used, the tundish slag thickness is 40-50mm, and the residual oxygen content of the tundish is 0.50%; argon flow control and other requirements for protecting each link of casting: the argon pipeline of the long shroud is opened, the argon flow rate is 180-200NL / min, and the back pressure is ≥0.2bar; the argon flow rate of the tundish upper shroud is 4-5NL / min, and the back pressure is 0.2bar; the stopper flow rate is 3-4NL / min, and the back pressure is 0.1bar; the argon blowing flow rate between plates is 5-6NL / min, and the back pressure is 0.1bar.

[0031] The chemical composition and mass percentage of the low-carbon high-chromium steel obtained in this embodiment are shown in Table 1, and the chemical composition of the low-carbon ferrochrome used is shown in Table 2.

[0032] Comparative Example 1: Based on the KR-BOF-RH-LF-CC process path, the specific process steps are described as follows.

[0033] KR desulfurization process: KR outgoing station S content is 0.0030%, and the slag bright surface area after desulfurization is 90%. BOF smelting process: BOF scrap ratio is 15%, the C content of hot metal entering the furnace is 4.3%, and argon is blown at the bottom throughout the process, and the bottom blowing gas supply intensity is 0.023~0.054Nm 3 / (min.t); BOF end oxygen level 450ppm, end temperature 1641℃. RH refining process: decarburization time 10min, carbon content 25ppm at the end of decarburization, no oxygen blowing to heat the molten steel after decarburization, pure circulation 4min after decarburization, minimum vacuum 3mbar; RH outlet temperature 1566℃, total oxygen in RH outlet steel 35ppm, total iron content in slag 0.8%. LF refining process: adopting micro-positive pressure operation in the furnace, slag thickness of 60mm, low-carbon ferrochrome added in batches, heating once every two batches of low-carbon ferrochrome 2.5t, alloying temperature of 1585-1598℃, bottom blowing flow of 800-1000NL / min, aluminum blocks and aluminum wires added in the last composition adjustment, feeding calcium wire after refining, calcium content of 0.0024%, feeding wire speed of 120m / min, calcium wire feeding angle of 85° with molten steel surface, soft blowing flow of 60NL / min, no exposure to molten steel; LF smelting cycle of 154min, power-on time of 57min, LF outlet temperature of 1577℃. Continuous casting process: the long water nozzle and gasket of the continuous casting ladle are intact, carbon-free tundish covering agent is used, tundish slag thickness is 30-35mm, and the residual oxygen content of the tundish is 4%. Argon flow control and other requirements for each link of protective casting: the long water inlet argon pipeline is opened, the argon flow rate is 150-185NL / min, and the back pressure is ≥0.2bar; the argon flow rate at the upper water inlet of the tundish is 3-5NL / min, and the back pressure is 0.3bar; the stopper flow rate is 3-4NL / min, and the back pressure is 0.2bar; the argon blowing flow rate between the plates is 4-5NL / min, and the back pressure is 0.2bar.

[0034] The chemical composition and mass percentage of the low-carbon high-chromium steel obtained in this comparative example are shown in Table 1, and the chemical composition of the low-carbon ferrochrome used is shown in Table 2.

[0035] Comparative Example 2: Based on the KR-BOF-RH-LF-CC process path, the specific process steps are described as follows.

[0036] KR desulfurization process: KR outgoing station S content is 0.0020%, and the slag bright surface area after desulfurization is 85%. BOF smelting process: BOF scrap ratio is 12%, the C content of hot metal entering the furnace is 4.2%, and argon is blown at the bottom throughout the process, and the bottom blowing gas supply intensity is 0.035~0.059Nm 3 / (min.t); BOF end oxygen level 747ppm, end temperature 1675℃. RH refining process: decarburization time 11min, carbon content 28ppm at the end of decarburization, minimum vacuum 4mbar, no oxygen blowing to heat the molten steel after decarburization, RH with aluminum particles for aluminum alloying, pure circulation 5min after decarburization; RH outlet temperature 1560℃, total oxygen in RH outlet steel 39ppm, total iron content in slag 0.7%. LF refining process: adopt micro-positive pressure operation in the furnace, slag thickness is 55mm, low-carbon ferrochrome is added in batches, each batch of low-carbon ferrochrome is heated once for 2.5t, the heating temperature is 1580-1590℃ for alloying, and the bottom blowing flow rate is 900-1000NL / min; after refining, calcium wire is fed, the calcium content is 0.0023%, the feeding wire speed is 140m / min, the calcium wire feeding angle is 90° with the steel liquid surface, the soft blowing flow rate is 55NL / min and the steel liquid cannot be exposed; LF smelting cycle is 157min, power-on time is 55min, and LF outlet temperature is 1574℃. Continuous casting process: The long shroud and its gasket of the continuous casting ladle are intact, a carbon-free tundish covering agent is used, the tundish slag thickness is 32-38mm, and the residual oxygen content of the tundish is 5%; argon flow control and other requirements for protecting each link of casting: the argon pipeline of the long shroud is opened, the argon flow rate is 120-17NL / min, and the back pressure is ≥0.1bar; the argon flow rate of the tundish upper shroud is 5-6NL / min, and the back pressure is 0.1bar; the stopper flow rate is 3-4NL / min, and the back pressure is 0.3bar; the argon blowing flow rate between the plates is 4-5NL / min, and the back pressure is 0.3bar.

[0037] The chemical composition and mass percentage of the low-carbon high-chromium steel obtained in this comparative example are shown in Table 1, and the chemical composition of the low-carbon ferrochrome used is shown in Table 2.

[0038] Table 1: Chemical composition (wt%) of low carbon high chromium steel obtained in Examples 1-4 and Comparative Examples 1-2

[0039] In Table 1, the remainder is Fe and inevitable impurity elements.

[0040] Table 2: Carbon, nitrogen and chromium contents (wt%) in low carbon ferrochrome used in Examples 1-4 and Comparative Examples 1-2

[0041] It can be seen from Table 1 and Table 2 that when the nitrogen content of the low-carbon ferrochrome used for alloying in the LF refining process is 0.025-0.030%, the nitrogen content of the low-carbon high-chromium steel obtained by this method is ≤66ppm, which is much lower than the nitrogen content of the low-carbon high-chromium steel obtained in the comparative example.

Claims

1. A smelting method for controlling nitrogen content in low-carbon high-chromium steel, characterized in that: It includes KR desulfurization, BOF smelting, RH refining, LF refining and continuous casting process; each process is as follows: The KR desulfurization process: adopts deep desulfurization mode, and the outgoing S content is ≤0.0015%; The BOF smelting process: the C content of the molten iron entering the furnace is ≥4.5%, the scrap ratio is ≤10%, and argon is blown at the bottom throughout the process; The RH refining process: oxygen blowing decarburization, the target carbon content after decarburization is ≤15ppm; after decarburization is completed, 500-100Nm 3 Oxygen heats up the molten steel; the total oxygen content in the RH steel is 150-300ppm, and the total iron content in the slag is 8-12%; The LF refining process: LF refining adopts a slightly positive pressure operation in the furnace, the slag thickness is 80-100mm, low carbon ferrochrome is added according to the target composition, the low carbon ferrochrome is added in batches, the temperature is raised once every 5-6t of low carbon ferrochrome is added, the alloying target temperature is 1580-1600°C, the bottom blowing flow rate is 500-600NL / min; after the refining is completed, the calcium wire is fed, and the feeding wire speed is 160-180m / min; The continuous casting process includes full protection casting and the residual oxygen content in the tundish is ≤0.50%.

2. The smelting method for controlling nitrogen content in low-carbon high-chromium steel according to claim 1, characterized in that: The BOF smelting process: the final oxygen level is controlled at 500-700 ppm, the final temperature is 1650-1670° C., high calcium lime and fluorite are added during the steelmaking process, and deoxidation and alloying are not performed.

3. The smelting method for controlling nitrogen content in low-carbon high-chromium steel according to claim 1, characterized in that: The RH refining process: pure circulation after decarburization ≥ 6 minutes, minimum vacuum ≤ 2 mbar, RH outlet temperature 1570 ~ 1580 ° C.

4. The smelting method for controlling nitrogen content in low-carbon high-chromium steel according to claim 1, characterized in that: The LF refining process: aluminum blocks and aluminum wires are added in the last composition adjustment, the soft blowing flow rate is 20-80NL / min and no molten steel is exposed, the LF smelting cycle is 100-120min, the power supply time is ≤50min, and the LF outlet temperature is 1570-1580°C.

5. A smelting method for controlling nitrogen content in low-carbon high-chromium steel according to any one of claims 1 to 4, characterized in that: The continuous casting process uses a carbon-free tundish covering agent, and the tundish slag thickness is 40 to 60 mm.