Hot-rolled wire rod for prestressed steel strand and preparation method of hot-rolled wire rod
Through the high-line rolling and controlled rolling and cooling process, the heating and threading temperature of the casting billet are controlled, combined with the segmented cooling technology, the problem of difficulty in producing ultra-high-strength prestressed steel strands in the existing technology is solved, and the problem of the existing technology is difficult to produce ultra-high-strength prestressed steel strands is realized. High-strength and low-cost production meets the performance requirements of high-end applications.
Patent Information
- Application Number
- CN202411216082.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The prior art is difficult to produce high-strength strips required for prestressed steel strands of ultra-high strength levels, and the production process is complex and costly, making it easy to produce harmful tissues that are not conducive to deep processing.
Using high-line rolling and controlled rolling and cooling processes, the prestressed steel stranded wire hot rolling disk with tensile strength ≥1960MPa was prepared through the control of the heating temperature, heating time, wire spinning temperature and segmented cooling technology. strip.
It realizes the production of prestressed steel strands with a simple process, easy to promote industrially, excellent product performance, and meets the needs of high-end applications.
Smart Images

Figure CN119020570A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wire rod production, and in particular to a hot-rolled wire rod for prestressed steel strands and a preparation method thereof. Background Art
[0002] Steel strand is a steel product made of multiple high-strength steel wires twisted in a spiral shape. The most commonly used are galvanized steel strand and prestressed steel strand. Prestressed steel strand is widely used in infrastructure. It is generally believed that the tensile strength of 1470-1860MPa is high-strength, and the tensile strength above 1860MPa is ultra-high-strength. At present, the main strength level used is 1860MPa, and the corresponding wire rod tensile strength is usually 1140-1200MPa. With the rapid development of industry, lightweight and high-strength have been extended to the steel strand industry.
[0003] Therefore, ultra-high-strength prestressed steel strands are in urgent need of development. Ultra-high-strength steel strands require higher-strength original wire rods, and alloying is one of the methods to improve the comprehensive performance of steel. An appropriate amount of alloying elements can be added to the steel to improve the strength and toughness of the steel. There are generally two options for the composition design of the wire rod: one is a high-carbon and high-silicon composition system with the addition of trace amounts of chromium; the other is a high-carbon system with the addition of various micro-alloying elements such as niobium, titanium, and vanadium. The addition of various micro-alloying elements such as niobium, titanium, and vanadium will result in relatively high alloy costs. At the same time, due to their low solubility in austenite, a higher soaking temperature is required during the heating process to dissolve them into austenite so that they can play a role in the subsequent rolling and cooling process. Therefore, it is more green and economical to adopt a high-carbon and high-silicon composition system.
[0004] The most effective way to increase the strength of the original wire rod is to increase the C content. However, if the C content is too high, the plasticity will be reduced, making it difficult to meet the subsequent production requirements of steel strands. Segregation is also prone to occur, which will lead to the formation of grain boundary cementite, martensite and other harmful structures that affect subsequent deep processing during the phase transformation after rolling, resulting in pull-out fracture. Si is a ferrite strengthening element with high solid solution strengthening ability. It can significantly improve the cold work hardening index of steel and reduce the strength loss during the heat treatment process. Therefore, by combining reasonable component design and production technology, hot-rolled wire rods that meet the ultra-high strength level of prestressed steel strands can be produced.
[0005] For example, the Chinese patent application number CN202011236089.3 discloses prestressed steel strands, wire rods for prestressed steel strands and their production methods. Specifically, it discloses that the wire rods for prestressed steel strands are prepared by sequentially performing the processes of molten iron pre-desulfurization, molten steel smelting, molten steel refining, continuous casting, high-wire rolling, temperature-controlled cooling and coiling. The finished product has a high carbon content and is difficult to control segregation. In the later stage, it is easy to produce harmful structures such as network carbides and martensite that are not conducive to drawing.
[0006] For example, a Chinese patent with application number CN202010503561.9 discloses a hot-rolled wire rod for ultra-high-strength steel strand and a preparation method thereof, which specifically discloses molten iron pretreatment - converter - refining - VD vacuum treatment - continuous casting - blanking - rolling, wherein: after the molten iron pretreatment process, the Si in the molten iron: 0.3~0.7%, S≤0.015%, P≤0.120%, Ti≤0.10%, T≥1250℃, and the wire rod prepared by this method belongs to the 1860MPa grade steel strand wire rod level, which cannot meet the subsequent development needs.
[0007] In view of this, the existing technology should be improved. Summary of the invention
[0008] The main purpose of the present invention is to provide a hot-rolled wire rod for prestressed steel strand and a preparation method thereof, which mainly includes high-speed wire rolling and controlled rolling and controlled cooling processes. By combining the heating temperature and heating time of the casting, the wire laying temperature control after rolling and the segmented controlled cooling technology, the hot-rolled wire rod for prestressed steel strand with good performance is finally obtained. The prestressed steel strand made of the wire rod has a tensile strength of ≥1960MPa and a maximum force total elongation (L 0 ≥500mm)Agt≥4.5%. This method has the advantages of simple process, low production cost and easy industrial promotion.
[0009] According to one aspect of the present invention, a method for preparing a hot-rolled wire rod for prestressed steel strand is proposed, which comprises: sequentially performing converter smelting, LF refining, and continuous casting to obtain the desired ingot, and then sequentially performing ingot heating, high-speed wire rolling, Stelmor air-cooling line controlled cooling, coiling and packaging to obtain the hot-rolled wire rod for prestressed steel strand; wherein, cooling is performed by a water tank before and after final rolling, the opening degree of the water tank before final rolling is greater than the opening degree of the water tank after final rolling, and in the controlled cooling process, the roller speed is increased step by step to a fixed value.
[0010] According to one embodiment of the present invention, the chemical composition of the hot-rolled wire rod for prestressed steel strand is as follows by weight percentage: C: 0.83% to 0.87%, Si: 0.50% to 0.60%, Mn: 0.60% to 0.80%, P≤0.015%, S≤0.010%, Cr: 0.25% to 0.35%, Cu≤0.20%, Ni≤0.10%; the rest is Fe and unavoidable impurities.
[0011] According to one embodiment of the present invention, in the high-speed wire rolling process, the soaking temperature of the ingot is 1080-1150° C., and the heating time t=(0.7-1.2)H, wherein H is the thickness of the ingot.
[0012] According to one embodiment of the present invention, the opening degree of the water tank before final rolling is ≥25%, and the water volume in the water tank is ≥50m 3 / h, outlet water pressure ≥3.5bar, temperature before final rolling is 860~880℃.
[0013] According to one embodiment of the present invention, after final rolling, the water tank opening degree is ≤5%, and the spinning temperature is controlled to be 880-900°C, and the temperature difference between the surface and the core of the wire rod is ≤10°C.
[0014] According to one embodiment of the present invention, the wire rod after spinning is controlled to be cooled in a Stelmor air cooling line, the initial roller speed is 0.50~0.60m / s, the roller speeds of the 2nd to 8th sections are increased step by step by 0.03~0.05m / s, and the roller speeds of the 9th to 13th sections are 0.74~1.00m / s.
[0015] According to one embodiment of the present invention, during the controlled cooling of the Stelmore air cooling line, the opening degree of the front fan is ≥60%, the thermal insulation cover is opened, the opening angle of the Jialing device is 2°~4°, and the temperature is quickly cooled to 580~620℃, and the temperature difference between the surface and the core of the wire rod is ≤15℃.
[0016] According to one embodiment of the present invention, the controlled cooling of the Stelmore air cooling line further includes: turning off the fan and the heat preservation cover, and slowly cooling at a cooling rate of 1 to 3°C / s, with a coiling temperature of 450 to 500°C.
[0017] According to another aspect of the present invention, a hot-rolled wire rod for prestressed steel strand is provided, which is prepared by any of the methods in the above technical solutions.
[0018] According to one embodiment of the present invention, the hot-rolled wire rod for prestressed steel strand has a troostite rate ≥ 95%, no central martensite, grain boundary cementite ≤ grade 1.0, a tensile strength ≥ 1250 MPa, and a cross-sectional shrinkage rate ≥ 30%.
[0019] In a preparation method of a hot-rolled wire rod for prestressed steel strand according to an embodiment of the present invention, the method mainly includes high-speed wire rolling and controlled rolling and controlled cooling processes. By combining the heating temperature and heating time of the casting, the wire laying temperature control after rolling and the segmented controlled cooling technology, the hot-rolled wire rod for prestressed steel strand with good performance is finally obtained. The prestressed steel strand made of the wire rod has a tensile strength of ≥1960MPa and a maximum force total elongation (L 0 ≥500mm)Agt≥4.5%. This method has the advantages of simple process, low production cost and easy industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment will be briefly introduced below. Obviously, the drawings described below are only some implementation cases of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 A process flow chart of a method for preparing a hot-rolled wire rod for prestressed steel strand according to an exemplary embodiment of the present invention is shown. DETAILED DESCRIPTION
[0022] The detailed description of the following embodiments is used to exemplify the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
[0023] The present invention provides these embodiments to make this disclosure thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.
[0024] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.
[0025] It should also be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.
[0026] All terms used in the present invention have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.
[0027] Technologies, methods, and apparatus known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, these technologies, methods, and apparatus should be considered part of the specification.
[0028] like Figure 1 As shown, the present invention provides a method for preparing a hot-rolled wire rod for prestressed steel strand, which comprises the following steps: S1, sequentially performing converter smelting, LF refining, and continuous casting to obtain the required ingot; S2, in turn, performs ingot heating, high-speed wire rolling, Stelmor air-cooling line controlled cooling, coiling and packaging to obtain hot-rolled wire rod for prestressed steel strand.
[0029] Among them, cooling is carried out through a water tank before and after the final rolling. The opening degree of the water tank before the final rolling is greater than the opening degree of the water tank after the final rolling. During the controlled cooling process, the roller speed is increased step by step to a fixed value.
[0030] In the preparation method of the hot-rolled wire rod for prestressed steel strand according to the embodiment of the present invention, it mainly includes high-speed wire rolling and controlled rolling and controlled cooling processes. By combining the heating temperature and heating time of the casting, the wire laying temperature control after rolling and the segmented controlled cooling technology, the hot-rolled wire rod for prestressed steel strand with good performance is finally obtained. The prestressed steel strand made of the wire rod has a tensile strength of ≥1960MPa and a maximum force total elongation (L 0 ≥500mm)Agt≥4.5%. This method has the advantages of simple process, low production cost and easy industrial promotion.
[0031] In some specific embodiments, the chemical composition of the hot-rolled wire rod for prestressed steel strands is as follows by weight percentage: C: 0.83% to 0.87%, Si: 0.50% to 0.60%, Mn: 0.60% to 0.80%, P≤0.015%, S≤0.010%, Cr: 0.25% to 0.35%, Cu≤0.20%, Ni≤0.10%; the rest is Fe and unavoidable impurities.
[0032] On the basis of the above embodiments, in the high-speed wire rolling process, the soaking temperature of the ingot is 1080-1150°C, and the heating time t=(0.7-1.2)H, where H is the thickness of the ingot.
[0033] In some specific embodiments, the water tank opening degree before final rolling is ≥25%, and the water volume in the water tank is ≥50m 3 / h, outlet water pressure ≥3.5bar, and temperature before final rolling is 860~880℃. By increasing the opening degree of the water tank before final rolling, the temperature of the rolled piece before entering the finishing mill can be effectively reduced, thereby more accurately controlling the final rolling temperature. This is especially important for steels that require a specific final rolling temperature to obtain ideal metallographic structure and mechanical properties. A larger opening degree means stronger cooling capacity, which helps to reduce temperature fluctuations caused by various factors (such as speed fluctuations, transportation time, etc.) during the rolling process and improve the stability of the final rolling temperature.
[0034] On the basis of the above embodiment, after final rolling, the water tank opening degree is ≤5%, and the spinning temperature is controlled to be 880-900°C, and the temperature difference between the surface and the core of the wire rod is ≤10°C.
[0035] In some specific embodiments, the wire rod after spinning is controlled to be cooled in a Stelmor air cooling line, the initial roller speed is 0.50-0.60 m / s, the roller speeds of the 2nd to 8th sections are increased step by step by 0.03-0.05 m / s, and the roller speeds of the 9th to 13th sections are 0.74-1.00 m / s.
[0036] The gradual increase in roller speed can ensure that the adjacent coils are gradually spaced apart during the air cooling process, reducing the heat transfer between the coils and thus improving the uniformity of cooling. By optimizing the roller speed, the grain size of the wire can be refined, thereby improving its tensile strength.
[0037] Specifically, the wire rod after spinning is controlled to be cooled in the Stelmore air cooling line, the initial roller speed is 0.56m / s, the roller speed of the 2nd to 8th sections increases by 0.04m / s step by step, and the roller speed of the 9th to 13th sections is 0.88m / s.
[0038] On the basis of the above embodiment, in the controlled cooling of the Stelmore air cooling line, the opening degree of the front fan is ≥60%, the heat preservation cover is opened, the opening angle of the Jialing device is 2°~4°, the temperature is quickly cooled to 580~620°C, and the temperature difference between the surface and the core of the wire rod is ≤15°C. Specifically, the opening angle of the Jialing device is 3°.
[0039] In some specific embodiments, the fan and the heat preservation cover are turned off, and slow cooling is performed at a cooling rate of 1 to 3° C. / s, and the coiling temperature is 450 to 500° C.
[0040] The present invention also provides a hot-rolled wire rod for prestressed steel strands, which is prepared by the method mentioned in the above technical solution.
[0041] In some specific embodiments, the hot-rolled wire rod for prestressed steel strand has a troostite ratio of ≥95%, no central martensite, grain boundary cementite ≤1.0 level, a tensile strength of ≥1250MPa, and a cross-sectional shrinkage of ≥30%.
[0042] This hot-rolled wire rod can be used to make 1×19S-21.8mm prestressed steel strand, with a tensile strength of ≥1960MPa and a maximum force total elongation (L 0 ≥500mm)Agt≥4.5%.
[0043] A specific application of the present invention is: The first step: the required ingot is obtained by converter smelting, LF refining and continuous casting. The composition of the ingot is C 0.83%-0.87%, Si 0.50%-0.60%, Mn 0.60%-0.80%, P≤0.015%, S≤0.010%, Cr 0.25%-0.30%, Cu≤0.20%, Ni≤0.10%, and the rest is Fe and unavoidable impurities.
[0044] Step 2: Heat the ingot with an average heating temperature of 1080-1150°C and a heating time of t=(0.7-1.2)H, where H is the thickness of the ingot. Then, dephosphorize the ingot with high-pressure water and roll it with a high-speed wire rolling unit.
[0045] (1) The water tank opening degree before final rolling is ≥25%, and the water volume in the water tank is ≥50m 3 / h, outlet water pressure ≥3.5bar, temperature before final rolling is 860~880℃; (2) After final rolling, the water tank opening degree is ≤5%, the spinning temperature is 880-900℃, the temperature difference between the surface and the core of the wire rod is ≤10℃, and the spinning speed is 30-35m / s.
[0046] Step 3: After spinning, the wire rod is cooled in sections on the Stelmore air cooling line. The cooling speed of the wire rod is controlled by controlling the opening value of the fan, the speed of the air cooling roller and the opening / closing of the insulation cover. The specific cooling control process is as follows: (1) Air-cooled roller speed control requirements: The first roller speed is 0.56 m / s, and increases by 0.04 m / s section by section; (2) Requirements for the opening of the fan, Jialing device and insulation cover: the opening degree of the front fan is ≥60%, the insulation cover is opened, the opening angle of the Jialing device is 3°, and the wire rod is quickly cooled to 580-620°C, and the temperature difference between the surface and the core of the wire rod is ≤15°C; then the fan and the insulation cover are turned off, and the wire rod is slowly cooled at a cooling rate of 1-3°C / s, and the coiling temperature is 450-500°C.
[0047] (3) By matching the Stelmor air cooling line fan, air cooling roller speed, Jialing device and insulation cover after rolling, the steel is first quickly cooled to 580-620°C after rolling to inhibit the formation of network cementite; then it is cooled at a cooling rate of 1-3°C / s to complete the troostite phase transformation and prevent the formation of abnormal martensite structure.
[0048] After the application of the present invention, the product quality fully meets the requirements of relevant technical conditions and has been sent to the user for deep processing. After meeting the user's requirements, the annual production volume is expected to be about 20,000 tons. The benefit per ton of steel is calculated at 200 yuan, which can create economic benefits of 4 million yuan. It can be promoted and applied in the production of hot-rolled wire rods and other high-carbon steels for high-strength prestressed steel strands in various steel plants, and has good promotion and application prospects.
[0049] The solution of the present application is described below through specific embodiments.
[0050] Example 1 A metal products company adopts the technology of the present invention to produce hot-rolled wire rod with a specification of φ14mm, 1×19S-21.8mm, 1960MPa for steel strands. The production process is: converter smelting → LF refining → continuous casting → billet heating → high-speed wire rolling → laying machine laying → Stelmor air-cooling line controlled cooling → coiling.
[0051] (1) The 200 mm x 200 mm ingot is produced by converter smelting, LF refining and continuous casting. The melting composition of the ingot is C: 0.83%, Si: 0.50%, Mn: 0.65%, P: 0.011%, S: 0.009%, Cr: 0.25%, Cu: 0.05%, Ni: 0.03%, and the rest is Fe and unavoidable impurities.
[0052] (2) Place the ingot into a walking beam heating furnace for heating. The heating temperature in the heating furnace soaking section is 1125°C and the heating time is 200 min.
[0053] (3) After phosphorus removal by high-pressure water, the steel is rolled into a φ14 mm round bar by a 30-stand high-wire rolling unit and then spun by a spinning machine. Before final rolling, the opening degrees of the 1# to 4# water tanks are 25%, 28%, 28% and 30% respectively, and the water inflow into the water tanks is 50, 55, 55 and 55 m3 respectively. 3 / h, the outlet water pressure is 3.5bar; the temperature before final rolling is 860℃; the water tank opening degree after final rolling is 3%, and the spinning temperature is 880℃.
[0054] (4) After spinning, the wire rod is controlled to cool in the Stelmor air cooling line. The specific control parameters are: the roller speed of the first section is 0.56 m / s, the roller speed of the second section is 0.60 m / s, the roller speed of the third section is 0.64 m / s, the roller speed of the fourth section is 0.68 m / s, the roller speed of the fifth section is 0.72 m / s, the roller speed of the sixth section is 0.76 m / s, and the roller speed of the seventh section is 0.80 m / s. m / s, the roller speed of the 8th roller is 0.84m / s, and the roller speed of the 9th to 13th rollers is 0.88m / s; the air volume of the 1st to 6th fans of the air cooling line is 100%, the air volume of the 7th to 8th fans is 90%, the opening value of the 9th fan is 70%, the opening value of the 10th fan is 60%, the 11th to 14th fans are closed, and the opening angle of the Jialing device is 3°; the 1st to 20th insulation covers are closed, the temperature entering the insulation covers is 580℃, and the winding temperature is 450℃.
[0055] (5) The φ14mm wire rod prepared by the above method has a tensile strength of 1250MPa, a cross-sectional shrinkage of ≥38%, a troostite rate of 95%, no central martensite, and a grain boundary cementite level of 0.5. The 1×19S-21.8mm prestressed steel strand made of the wire rod has a tensile strength of 1960MPa and a maximum force total elongation (L 0 ≥500mm)Agt≥5.1%.
[0056] Example 2 A metal products company adopts the technology of the present invention to produce hot-rolled wire rod with a specification of φ14mm, 1×19S-21.8mm: 1960MPa for steel strands. The production process is: converter smelting → LF refining → continuous casting → billet heating → high-speed wire rolling → wire laying machine spinning → Stelmor air-cooling line controlled cooling → coiling.
[0057] (1) The 200 mm x 200 mm ingot is produced by converter smelting, LF refining and continuous casting. The melting composition of the ingot is C: 0.87%, Si: 0.60%, Mn: 0.80%, P: 0.013%, S: 0.008%, Cr: 0.35%, Cu: 0.02%, Ni: 0.03%, and the rest is Fe and unavoidable impurities.
[0058] (2) Place the ingot into a walking beam heating furnace for heating. The soaking temperature of the heating furnace is 1150°C and the heating time is 200 min.
[0059] (3) After dephosphorization by high-pressure water, the steel is rolled into a φ14 mm round bar by a 30-stand high-wire rolling unit and then spun by a spinning machine. Before final rolling, the opening degrees of the 1# to 4# water tanks are 25%, 28%, 28% and 30% respectively, and the water inflow into the water tanks is 50, 55, 55 and 55 m3 respectively. 3 / h, the outlet water pressure is 3.5bar; the temperature before final rolling is 880℃; the water tank opening degree after final rolling is 3%, and the spinning temperature is 900℃.
[0060] (4) After spinning, the wire rod is controlled to cool in the Stelmor air cooling line. The specific control parameters are: the roller speed of the first section is 0.56 m / s, the roller speed of the second section is 0.60 m / s, the roller speed of the third section is 0.64 m / s, the roller speed of the fourth section is 0.68 m / s, the roller speed of the fifth section is 0.72 m / s, the roller speed of the sixth section is 0.76 m / s, and the roller speed of the seventh section is 0.80 m / s. m / s, the roller speed of the 8th roller is 0.84m / s, and the roller speed of the 9th to 13th rollers is 0.88m / s; the air volume of the 1st to 6th fans of the air cooling line is 100%, the air volume of the 7th to 8th fans is 90%, the opening value of the 9th fan is 70%, the opening value of the 10th fan is 60%, the 11th to 14th fans are closed, and the opening angle of the Jialing device is 3°; the 1st to 20th insulation covers are closed, the temperature entering the insulation covers is 620℃, and the winding temperature is 500℃.
[0061] (5) The φ14mm wire rod prepared by the above method has a tensile strength of 1310MPa, a cross-sectional shrinkage of ≥35%, a troostite ratio of 96%, no central martensite, and a grain boundary cementite level of 1.0. The 1×19S-21.8mm prestressed steel strand made of the wire rod has a tensile strength of 2100MPa and a maximum force total elongation (L 0 ≥500mm)Agt≥4.5%.
[0062] Example 3 A metal products company adopts the technology of the present invention to produce hot-rolled wire rod with a specification of φ14mm, 1×19S-21.8mm: 1960MPa for steel strands. The production process is: converter smelting → LF refining → continuous casting → billet heating → high-speed wire rolling → wire laying machine spinning → Stelmor air-cooling line controlled cooling → coiling.
[0063] (1) The 200 mm x 200 mm ingot is produced by converter smelting, LF refining and continuous casting. The melting composition of the ingot is C: 0.85%, Si: 0.56%, Mn: 0.71%, P: 0.015%, S: 0.008%, Cr: 0.27%, Cu: 0.02%, Ni: 0.03%, and the rest is Fe and unavoidable impurities.
[0064] (2) Place the ingot into a walking beam heating furnace for heating. The heating temperature in the heating furnace soaking section is 1080°C and the heating time is 200 min.
[0065] (3) After dephosphorization by high-pressure water, the steel is rolled into a φ14 mm round bar by a 30-stand high-wire rolling unit and then spun by a spinning machine. Before final rolling, the opening degrees of the 1# to 4# water tanks are 25%, 28%, 28% and 30% respectively, and the water inflow into the water tanks is 50, 55, 55 and 55 m3 respectively. 3 / h, the outlet water pressure is 3.5bar; the temperature before final rolling is 870℃; the water tank opening degree after final rolling is 3%, and the spinning temperature is 891℃.
[0066] (4) After spinning, the wire rod is controlled to cool in the Stelmor air cooling line. The specific control parameters are: the roller speed of the first section is 0.56 m / s, the roller speed of the second section is 0.60 m / s, the roller speed of the third section is 0.64 m / s, the roller speed of the fourth section is 0.68 m / s, the roller speed of the fifth section is 0.72 m / s, the roller speed of the sixth section is 0.76 m / s, and the roller speed of the seventh section is 0.80 m / s. m / s, the roller speed of the 8th roller is 0.84m / s, and the roller speed of the 9th to 13th rollers is 0.88m / s; the air volume of the 1st to 6th fans of the air cooling line is 100%, the air volume of the 7th to 8th fans is 90%, the opening value of the 9th fan is 70%, the opening value of the 10th fan is 60%, the 11th to 14th fans are closed, and the opening angle of the Jialing device is 3°; the 1st to 20th insulation covers are closed, the temperature entering the insulation covers is 598℃, and the rolling temperature is 482℃.
[0067] (5) The φ14mm wire rod prepared by the above method has a tensile strength of 1289MPa, a cross-sectional shrinkage of ≥36%, a troostite rate of 96%, no central martensite, and a grain boundary cementite level of 0.5. The 1×19S-21.8mm prestressed steel strand made of the wire rod has a tensile strength of 2080MPa and a maximum force total elongation (L 0 ≥500mm)Agt≥4.6%.
[0068] After the implementation of the present invention, at least the following beneficial effects are achieved: The high-speed wire rolling and controlled rolling and controlled cooling processes achieve comprehensive optimization of the hot-rolled wire rod production process by finely controlling the heating temperature and heating time of the ingot, as well as the strict control of the wire drawing temperature after rolling, combined with advanced segmented controlled cooling technology. This series of precise process measures ensures that the hot-rolled wire rods obtained in the end have excellent performance in mechanical properties, dimensional accuracy, surface quality and other aspects, meeting the strict requirements of high-end application fields. This production method not only has a simple and clear process flow and is easy to operate and manage, but also effectively reduces production costs and improves production efficiency, making this high-quality hot-rolled wire rod production technology easier to promote and apply in industrial production, which is of great significance to improving the production level and product quality of the entire industry.
[0069] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is for description only and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including the claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.
[0070] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for preparing a hot-rolled wire rod for prestressed steel strand, characterized in that: include: The converter smelting, LF refining and continuous casting are carried out in sequence to obtain the required ingots, and then the ingots are heated, high-speed wire rolled, Stelmor air-cooling line controlled cooling, coiled and packaged in sequence to obtain hot-rolled wire rods for prestressed steel strands; wherein, cooling is carried out through a water tank before and after the final rolling, and the opening degree of the water tank before the final rolling is greater than the opening degree of the water tank after the final rolling. In the controlled cooling process, the roller speed is increased step by step to a fixed value.
2. The method for preparing the hot-rolled wire rod for prestressed steel strand according to claim 1, characterized in that: The chemical composition of the hot-rolled wire rod for prestressed steel strands is as follows by weight percentage: C: 0.83% to 0.87%, Si: 0.50% to 0.60%, Mn: 0.60% to 0.80%, P≤0.015%, S≤0.010%, Cr: 0.25% to 0.35%, Cu≤0.20%, Ni≤0.10%; the rest is Fe and unavoidable impurities.
3. The method for preparing the hot-rolled wire rod for prestressed steel strand according to claim 1, characterized in that: In the high-speed wire rolling process, the soaking temperature of the ingot is 1080-1150° C., and the heating time is t=(0.7-1.2)H, where H is the thickness of the ingot.
4. The method for preparing the hot-rolled wire rod for prestressed steel strand according to claim 1, characterized in that: The opening degree of the water tank before final rolling is ≥25%, and the water volume in the water tank is ≥50m 3 / h, outlet water pressure ≥3.5bar, temperature before final rolling is 860~880℃.
5. The method for preparing the hot-rolled wire rod for prestressed steel strand according to claim 4, characterized in that: After final rolling, the water tank opening degree is ≤5%, and the spinning temperature is controlled at 880-900℃, and the temperature difference between the surface and the core of the wire rod is ≤10℃.
6. The method for preparing the hot-rolled wire rod for prestressed steel strand according to claim 5, characterized in that: The wire rod after spinning is controlled to be cooled in the Stelmor air cooling line, the initial roller speed is 0.50-0.60 m / s, the roller speeds of the 2nd to 8th sections are increased step by step by 0.03-0.05 m / s, and the roller speeds of the 9th to 13th sections are 0.74-1.00 m / s.
7. The method for preparing hot-rolled wire rod for prestressed steel strand according to claim 1, characterized in that: During the controlled cooling of the Stelmore air cooling line, the opening degree of the front fan is ≥60%, the insulation cover is opened, the opening angle of the Jialing device is 2°~4°, and the temperature is quickly cooled to 580~620℃, and the temperature difference between the surface and the core of the wire rod is ≤15℃.
8. The method for preparing the hot-rolled wire rod for prestressed steel strand according to claim 7, characterized in that: The controlled cooling of the Stelmore air cooling line also includes: turning off the fan and the heat preservation cover, slowly cooling at a cooling rate of 1 to 3°C / s, and the coiling temperature is 450 to 500°C.
9. A hot-rolled wire rod for prestressed steel strand, characterized in that: The method is prepared by any one of claims 1 to 8.
10. The hot rolled wire rod for prestressed steel strand according to claim 9, characterized in that: The hot-rolled wire rod for the prestressed steel strand has a troostite rate of ≥95%, no central martensite, grain boundary cementite ≤1.0 level, a tensile strength of ≥1250MPa, and a cross-sectional shrinkage of ≥30%.
Citation Information
Patent Citations
Controlled rolling and controlled cooling method for reducing martensite in microstructure of high-alloy steel hot-rolled wire rod
CN112239803A
Hot-rolled wire rod for high-strength low-relaxation prestressed steel strand and preparation method of hot-rolled wire rod
CN113981312A
SWRH82B hot-rolled wire rod with nominal diameter of 12.5 mm for prestressed steel strand, and preparation method thereof
CN114000048A
Ultrahigh-strength 85-grade tire cord steel wire rod and production method thereof
CN115976415A
Rolling controlled cooling method for reducing network cementite of SWRH82B hot-rolled wire rod
CN116000109A
Cited By
Production method of annealing-free cold forging steel hot-rolled wire rod
CN120169825A
Production method and application of hot-rolled wire rod for high-strength and high-plasticity steel wire rope
CN121198764A