Production method of high-magnesium fluxed chromium ore pellets

By adding magnesite powder and dolomite powder to chromium powder, the crystal structure and porosity of the pellets are changed, and the problem of easy and difficult reduction of chromium powder pellets in South Africa is solved, and the chromium harvest rate and smelting efficiency are improved. Reduces smelting power consumption.

CN119020587APending Publication Date: 2024-11-26SHANXI TAIGANG WANBANG CHARGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411146574.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the smelting process, the oxidative pellets have poor melting and difficult reduction performance, resulting in poor furnace stability, low chromium yield, and high smelting power consumption.

Method used

Add magnesite powder and dolomite powder to chromium ore powder to change the crystal structure of the pellet through high-temperature decomposition reaction, increase porosity and flux distribution uniformity, improve the magnesium-aluminum ratio, improve the reduction and reaction performance of the pellet, and reduce smelting During the process, the amount of flux is added and the heat of decomposition.

Benefits of technology

It improves the reduction performance and chromium harvesting rate of chromium ore pellets, reduces the smelting power consumption, avoids decomposition and heat absorption during the smelting process, and improves the meltability and smelting efficiency of the pellets.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of iron alloy raw material pellet production, in particular to a production method of high-magnesium fluxed chromium ore pellets, which comprises the following steps: adding magnesite powder and dolomite powder into chromium ore powder, so that the main indexes of the chromium ore powder pellets meet the specified requirements, and carrying out decomposition reaction on the added materials at high temperature in a roasting furnace to obtain the high-magnesium fluxed chromium ore pellets. The dislocations and defects of the grain structure of the chromium ore powder are increased, the pellet porosity is improved, uniform distribution of the flux and the chromium ore in the pellets is achieved, the reduction performance of the chromium ore pellets is improved, the chromium recovery rate of the chromium pellets in the smelting process is improved, and smelting power consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ferroalloy raw material pellet production, and in particular to a method for producing high-magnesium flux chromite pellets. Background Art

[0002] As the main chrome ore producing countries in the world have tightened restrictions on the export of raw materials, the global chromium ore resources available for circulation are decreasing. At present, the mainstream chromium ore resources on the market are South African chrome concentrate powder. The roasted pellets of South African chrome ore powder have become the main raw material for ferrochrome smelting. South African chrome ore powder has a low magnesium-aluminum ratio and is a smeltable and difficult-to-reduce ore. The oxidizing pellets produced mainly with it have poor reduction performance. Although a variety of fluxes are added during the smelting process, there are still problems such as poor furnace stability, high chromium content in the slag, and low chromium recovery rate.

[0003] Aiming at the characteristics of oxidized pellets produced by South African chrome ore powder being easy to melt and difficult to reduce, the present invention changes the crystal structure of chrome ore powder pellets by adding magnesite powder and dolomite powder to the ore powder, utilizing the decomposition reaction of magnesite powder and dolomite powder at high temperature in the roasting furnace and the oxidation reaction of chrome ore pellets, and increases the number of dislocations and defects between grains. At the same time, due to the release of part of the gas by the decomposition reaction of magnesite powder and dolomite powder, the porosity of the pellets is increased, and the reduction performance and reaction performance of the chrome ore pellets are improved. The method of adding high-magnesium flux to the pellets is adopted to achieve uniform distribution of the flux, effectively improve the reaction performance during the pellet smelting process, and reduce the amount of flux added during the smelting process. At the same time, since the flux has completed the decomposition reaction in the pellet roasting stage, there is no need to perform the decomposition reaction during the smelting process, avoiding the decomposition endothermic heat in the smelting stage, and reducing the smelting power consumption. The method of adding high-magnesium flux to the pellets improves the magnesium-aluminum ratio of the pellets, changes the melting range of the pellet reaction, and improves the problem that the pellets are easy to melt and difficult to reduce. In the process of pellet production, flux is reasonably added to produce high-magnesium flux pellets and effectively improve the yield of chrome ore pellets in the smelting process. Summary of the invention

[0004] The purpose of the present invention is to provide a method for producing high-magnesium flux chromium ore pellets in view of the above problems.

[0005] The object of the present invention is achieved as follows: A method for producing high-magnesium flux chromium ore pellets, comprising the following steps: Step 1: Batching: Adding magnesite powder and dolomite powder bins to the primary batching system for roasting, the dolomite powder index: particle size: ≤5mm, MgO: 18-22%, CaO: 28-32%; the magnesite powder index: particle size: ≤5mm, MgO: 42-46%; according to the MgO, Al2O3 and SiO2 content of the comprehensive ore powder, the comprehensive ore powder after adding dolomite powder and magnesite powder is controlled to have the following content: M / A: 0.85-0.95, CaO: 0.5-2.5%, SiO2: 4.5-6. 5%; Step 2: Ball milling: According to the theoretical calculation of the proportion of mineral powder, dolomite powder, magnesite powder and coke powder, the proportion of magnesite powder and dolomite powder mixture is 3%-10%, and the rest is mineral powder; coke powder is 2%-5% according to the amount of magnesite powder and dolomite powder mixture. After mixing, the fixed carbon content of the raw ball is 1.8%-2.8%, and the magnesium-aluminum ratio of the ball is 0.8-0.95. The wet overflow ball mill is fed according to the set value of the primary feed rate of 95-110t / h. The water amount is automatically calculated and added according to the slurry concentration to control the slurry concentration to 73%-76%. Steel balls are added to control the ball mill power at 2000-2600kwh. The pulp mass fraction is between 73% and 76%, ensuring that the particle size of the pulp after ball milling is as follows: -200 mesh: 79-83%, -325 mesh: 60-68%, -400 mesh: 45-53%; Step 3: Ceramic dehydration: The pulp that meets the above particle size levels is dehydrated with a ceramic filtration system, and the filter cake thickness is controlled at 12-15mm, and the filter cake moisture content is controlled at 9.0-10.0%; Step 4: Mixing and balling: In the secondary batching system, the dehydrated filter cake is proportionally added with fine powder return material and bentonite, mixed by a strong mixer, and then added to the drum balling machine to produce raw pellets and control the raw balls. The ball diameter is 8-16mm, the wet strength of the raw pellets is controlled at 1.0-1.5kg / ball, and the dry strength of the raw pellets is controlled at 5-10kg / ball; Step 5: Distribution and roasting: The raw pellets are operated by a shuttle distribution belt conveyor and a wide belt feeder to form a standardized material surface, that is, the material surface is flat, the thickness is uniform, the cross-section is a regular isosceles trapezoid, and the material surface has no pits, holes, grooves and other uneven structures. The crushed particle material is then returned to the drum pelletizing machine through a roller distributor for re-pelletizing. Qualified raw pellets fall on the steel belt that has been laid with the base material, and enter the roasting furnace at a speed of 0.6-0.8m / min for drying, preheating, roasting and cooling to finally obtain finished pellets.

[0006] In the step 1, one or both of dolomite powder and magnesite powder can be added.

[0007] The material level of the intensive mixer in step 4 is controlled at 3.5-4.5t to ensure that the materials are mixed evenly in the intensive mixer and the moisture content of the materials is controlled between 10.0% and 10.8%.

[0008] In the step 4, 0-30 kg / t of fine powder return material, 11-13.5 kg / t of bentonite, and the moisture content of the raw pellets are 10.0-10.5%.

[0009] In step 5, the drying temperature is 380-500°C, and the air volume is the amount of air entering the furnace × (800-1000) Nm 3 / h, preheating temperature: 1050~1150℃, air volume: furnace volume × (450~550) Nm 3 / h, roasting section temperature: 1150~1250℃, air volume: furnace volume×(300~450)Nm 3 / h.

[0010] The beneficial effects of the present invention are as follows: by adding dolomite powder and magnesite powder to the primary batching system, after the high-temperature reaction occurs between the powder and the chrome ore powder in the roasting furnace, the contents of MgO, CaO and SiO2 in the pellets are increased, the crystal structure of the chrome ore powder is changed, the dislocation and defects of the chrome ore powder crystals are increased, and the reduction performance of the chromium element in the crystals is improved. At the same time, due to the release of part of the gas by the decomposition reaction of the magnesite powder and the dolomite powder, the porosity of the pellets is increased, and the reduction performance and reaction performance of the chrome ore pellets are improved. The method of adding high-magnesium flux to the pellets achieves uniform distribution of the flux, effectively improves the reaction performance during the pellet smelting process, and reduces the amount of flux added during the smelting process. At the same time, since the flux has completed the decomposition reaction in the pellet roasting stage, there is no need to perform the decomposition reaction during the smelting process, avoiding the decomposition endothermic heat in the smelting stage, and reducing the smelting power consumption. The method of adding high-magnesium flux to the pellets improves the magnesium-aluminum ratio of the pellets, changes the melting range of the pellet reaction, and improves the problem that the pellets are easy to melt and difficult to reduce. In the process of pellet production, flux is reasonably added to produce high-magnesium flux pellets and effectively improve the yield of chrome ore pellets in the smelting process. DETAILED DESCRIPTION

[0011] The present invention adopts the following technical scheme: S1: Batching: Add magnesite powder and dolomite powder bins to the roasting primary batching system (use the existing system, no new equipment is needed, the primary batching bin is a cement bin, and batching is achieved by combining a disc feeder and a belt scale. The disc feeder model is: 5PKC315N; the belt scale model is: ISC-800-DL (3500A); vacate a primary batching bin for adding magnesite powder and dolomite powder, and the two are first evenly mixed in a certain proportion in the raw material yard. After mixing, the materials are fed into the same bin for production.) The main indicators of dolomite powder are: particle size: ≤5mm, MgO: 18-22%, CaO: 28-32%; the main indicators of magnesite powder are: particle size: ≤5mm, MgO: 42-46%; according to the content of MgO, Al2O3 and SiO2 in the comprehensive mineral powder, the comprehensive mineral powder after adding dolomite powder and magnesite powder is controlled to have: M / A: 0.85~0.95, CaO: 0.5~2.5%, SiO2: 4.5-6.5%.

[0012] S2: Ball milling: According to the theoretical calculation of the proportion of mineral powder, dolomite powder, magnesite powder and coke powder, the proportion of magnesite powder and dolomite powder mixture is 3%-10%, and the rest is mineral powder. The proportion of coke powder is 2%-5% according to the amount of magnesite powder and dolomite powder mixture. After mixing, the fixed carbon content of raw balls is 1.8%-2.8%, and the magnesium-aluminum ratio of pellets is 0.8-0.95. The wet overflow ball mill is fed according to the set value of 95-110t / h of the primary feed rate. The water amount is automatically calculated and added according to the slurry concentration to control the ore. The slurry concentration is 73%-76%, that is, 31 tons to 37 tons of water are added for every 100 tons of mineral powder. The ball mill power is controlled at 2000-2600kwh by adding steel balls, and the slurry mass fraction is between 79 and 83%. The particle size of the slurry after ball milling is ensured to be as follows: -200 mesh: 79-83%, -325 mesh: 60-68%, -400 mesh: 45-53%. The residence time of the material in the ball mill and the grinding efficiency are adjusted by controlling the feed amount and the amount of grinding balls added, so that the particle size of the material after grinding finally meets the standard.

[0013] S3: Ceramic dehydration: Ceramic filtration system for slurry that meets the above particle size grades (named as ceramic filter, filtration area 80m 2 ) for dehydration treatment, and by controlling the vacuum degree, rotation speed and liquid level of the slurry tank of the ceramic filter, the filter cake thickness is controlled at 12-15mm and the filter cake moisture content is controlled at 9.0-10.0%.

[0014] S4: Mixing and pelletizing: In the secondary batching system (using the existing secondary batching system, the specific silo is a steel silo structure, and the material is discharged by a combination of a disc feeder and a belt scale. The disc feeder model is: 5PKC315N; the belt scale model is: ISC-800-DL (3500A)), the dehydrated filter cake is proportionally mixed with fine powder return material and bentonite, mixed by a high-power mixer, and then added to the drum pelletizing machine to produce raw pellets with particle size and strength that meet the requirements, and the raw ball diameter is controlled to be 8-16mm, the raw ball strength is controlled to be 1.0-1.5kg / ball, and the raw ball dry strength is controlled to be 5-10kg / ball.

[0015] S5: Distribution and roasting: The raw pellets are operated by shuttle distribution belt conveyors and wide belt feeders to form a standardized material surface (the material surface is flat, the thickness is uniform, the cross-section is a regular isosceles trapezoid, and there are no pits, holes, grooves and other uneven structures on the material surface). The crushed particle material is then returned to the pelletizing system through a roller distributor. Qualified raw pellets fall on the steel belt that has been laid with the base material, and enter the roasting furnace at a speed of 0.6-0.8m / min for drying, preheating, roasting and cooling to finally obtain finished pellets.

[0016] In the step S1, one or both of dolomite powder and magnesite powder can be added according to comprehensive mineral powder indicators.

[0017] The material level of the mixer in step S4 is controlled at 3.5-4.5t to ensure that the materials are evenly mixed in the mixer and the moisture content of the materials is controlled between 10.0% and 10.8%. Mixer model: DW 29 / 4 conti, capacity is 5 tons, hourly processing capacity of the mixer is 110t / h, and water distribution capacity is 0-2000L / h.

[0018] In the step S4, 0-30 kg / t of fine powder return material, 11-13.5 kg / t of bentonite, 10.0-10.5% of raw ball moisture, and 8-16 mm of raw ball particle size are added.

[0019] In step S5, the temperature of the drying section is 380-500°C, the air volume is the amount of air entering the furnace × (800-1000) Nm3 / h, the temperature of the preheating section is 1050-1150°C, the air volume is the amount of air entering the furnace × (450-550) Nm3 / h, the temperature of the roasting section is 1150-1250°C, the air volume is the amount of air entering the furnace × (300-450) Nm3 / h. The green balls stay in the drying section for about 7.3 minutes, the heating and roasting sections stay for about 5.3 minutes each, the balance section stays for about 4 minutes, and the three cooling sections stay for about 18 minutes. After the balls are cooled, the finished balls are obtained. Embodiment 1

[0020] A method for producing high-magnesium flux chrome ore pellets, which specifically comprises the following steps: adding magnesite powder and dolomite powder bins to a roasting primary batching system, wherein the main indicators of the dolomite powder are as follows: particle size 0-5 mm: 95.50%, MgO: 21.04%, and CaO: 29.93%; the main indicators of the magnesite powder are as follows: particle size 0-5 mm: 99.59%, and MgO: 45.49%; and according to the MgO, Al2O3, and SiO2 contents of the comprehensive ore powder, the comprehensive ore powder after adding dolomite powder and magnesite powder is controlled to have the following contents: M / A: 0.91, CaO: 1.87%, and SiO2: 6.45%.

[0021] S2: Ball milling: According to the theoretically calculated proportion of mineral powder, dolomite powder, magnesite powder and coke powder, the wet overflow ball mill is fed at a set value of 107t / h at a time, the carbon setting value is fixed at 2.4%, the total proportion of dolomite powder and magnesite powder is 10%, and the water amount is automatically calculated and added according to the slurry concentration. The ball mill power is controlled at 2200kw by adding steel balls, and the slurry mass fraction is about 74.6%, ensuring that the slurry particle size after ball milling is as follows: -200 mesh: 79~83%, -325 mesh: 60~68%, -400 mesh: 45~53%. The residence time of the material in the ball mill and the grinding efficiency are adjusted by controlling the feed amount and the amount of grinding balls added, so that the particle size of the material after grinding finally meets the standard.

[0022] S3: Ceramic dehydration: The slurry that meets the above-mentioned particle size level is dehydrated by a ceramic filtration system. By controlling the vacuum degree, rotation speed and liquid level of the slurry tank of the ceramic filter, the filter cake thickness is controlled at 12mm and the water content of the filter cake is controlled at about 9.6%.

[0023] S4: Mixing and pelletizing: In the secondary batching system, the dehydrated filter cake is mixed with fine powder return material and bentonite in proportion, mixed by a strong mixer, and then added to the drum pelletizing machine to produce green pellets with particle size and strength that meet the requirements, with the green ball diameter controlled at 8-16mm, the green ball strength controlled at 1.3kg / ball, and the green ball dry strength controlled at 5.5kg / ball.

[0024] S5: Distribution and roasting: The raw pellets are formed into a standardized material surface through the operation of shuttle distribution belt conveyor and wide belt feeder, and then the crushed granular materials are returned to the pelletizing system through the roller distributor. The qualified raw pellets fall on the steel belt with the bottom material laid, and enter the roasting furnace at a speed of about 0.73m / min for drying, preheating, roasting and cooling, and finally the finished pellets are obtained.

[0025] In the step S1, the dolomite powder and the magnesite powder are added in a ratio of dolomite powder to magnesite powder = 52:48 according to the comprehensive mineral powder index.

[0026] The material level of the mixer in step S4 is controlled at 3.5t to ensure that the materials are mixed evenly in the mixer and the moisture content of the materials is controlled at about 10.5%.

[0027] In step S4, 28 kg / t of fine powder return material and 11.5 kg / t of bentonite are added, the moisture content of the raw balls is 10.5%, and the particle size of the raw balls is 10-16 mm.

[0028] In step S5, the drying temperature is 380-450°C, and the air volume is 84000 Nm 3 / h, preheating temperature: 1050~1150℃, air volume: 41400Nm 3 / h, roasting section temperature: 1150~1250℃, air volume: 27500Nm 3 / h or so.

[0029] With the optimized process, the chromium recovery rate of chrome ore pellets can be increased by 0.5 percentage points during the smelting process, and the Cr2O3 content in the slag has been reduced from the previous average of 8.5-10.5% to the current 7-8.5%. The smelting power consumption has been reduced from 3419kwh / t to 3317kwh / t. Embodiment 2

[0030] A method for producing high-magnesium flux chrome ore pellets, which specifically comprises the following steps: adding magnesite powder and dolomite powder bins to a roasting primary batching system, wherein the main indicators of the dolomite powder are as follows: particle size 0-5 mm: 95.50%, MgO: 21.04%, and CaO: 29.93%; the main indicators of the magnesite powder are as follows: particle size 0-5 mm: 99.59%, and MgO: 45.49%; and according to the MgO, Al2O3, and SiO2 contents of the comprehensive ore powder, the comprehensive ore powder after adding dolomite powder and magnesite powder is controlled to have the following contents: M / A: 0.85, CaO: 1.46%, and SiO2: 6.50%.

[0031] S2: Ball milling: According to the theoretically calculated proportion of mineral powder, dolomite powder, magnesite powder and coke powder, the wet overflow ball mill is fed at a set value of 107t / h at a time, the carbon setting value is fixed at 2.25%, the total proportion of dolomite powder and magnesite powder is 4-6%, and the water amount is automatically calculated and added according to the slurry concentration. The ball mill power is controlled at 2200kw by adding steel balls, and the slurry mass fraction is about 74.6%, ensuring that the slurry particle size after ball milling is as follows: -200 mesh: 79~83%, -325 mesh: 60~68%, -400 mesh: 45~53%. The residence time of the material in the ball mill and the grinding efficiency are adjusted by controlling the feed amount and the amount of grinding balls added, and finally the particle size of the material after grinding meets the standard.

[0032] S3: Ceramic dehydration: The slurry that meets the above-mentioned particle size level is dehydrated by a ceramic filtration system. By controlling the vacuum degree, rotation speed and liquid level of the slurry tank of the ceramic filter, the filter cake thickness is controlled at 12mm and the water content of the filter cake is controlled at about 9.6%.

[0033] S4: Mixing and pelletizing: In the secondary batching system, the dehydrated filter cake is mixed with fine powder return material and bentonite in proportion, mixed by a strong mixer, and then added to the drum pelletizing machine to produce green pellets with particle size and strength that meet the requirements, with the green ball diameter controlled at 8-16mm, the green ball strength controlled at 1.3kg / ball, and the green ball dry strength controlled at 5.5kg / ball.

[0034] S5: Distribution and roasting: The raw pellets are formed into a standardized material surface through the operation of shuttle distribution belt conveyor and wide belt feeder, and then the crushed granular materials are returned to the pelletizing system through the roller distributor. The qualified raw pellets fall on the steel belt with the base material laid on it, and enter the roasting furnace at a speed of about 0.75m / min for drying, preheating, roasting and cooling, and finally the finished pellets are obtained.

[0035] In the step S1, the dolomite powder and the magnesite powder are added in a ratio of dolomite powder to magnesite powder = 52:48 according to the comprehensive mineral powder index.

[0036] The material level of the mixer in step S4 is controlled at 3.5t to ensure that the materials are mixed evenly in the mixer and the moisture content of the materials is controlled at about 10.5%.

[0037] In step S4, 28 kg / t of fine powder return material and 11.5 kg / t of bentonite are added, the moisture content of the raw balls is 10.5%, and the particle size of the raw balls is 10-16 mm.

[0038] In step S5, the drying temperature is 380-450°C, and the air volume is 84000 Nm 3 / h, preheating temperature: 1050~1150℃, air volume: 41400Nm 3 / h, roasting section temperature: 1150~1250℃, air volume: 27500Nm 3 / h or so.

[0039] With the optimized process, the chromium recovery rate of chrome ore pellets can be increased by 0.5 percentage points during the smelting process, and the Cr2O3 content in the slag has been reduced from the previous average of 8.5-10.5% to the current 8.1-8.8%. The smelting power consumption has been reduced from 3419kwh / t to 3276kwh / t.

[0040] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.

Claims

1. A method for producing high-magnesium flux chromium ore pellets, characterized in that: The following steps are involved: Step 1: Batching: Add magnesite powder and dolomite powder bins to the roasting batching system. Dolomite powder index: particle size: ≤5mm, MgO: 18-22%, CaO: 28-32%; magnesite powder index: particle size: ≤5mm, MgO: 42-46%; According to the content of MgO, Al2O3 and SiO2 in the comprehensive mineral powder, the comprehensive mineral powder after adding dolomite powder and magnesite powder is controlled to have the following content: M / A: 0.85-0.95, CaO: 0.5-2.5%, SiO2: 4.5-6.5%; Step 2: Ball milling: According to the theoretically calculated proportion of mineral powder, dolomite powder, magnesite powder and coke powder, the proportion of magnesite powder and dolomite powder mixture is 3%-10%, and the rest is mineral powder; coke powder is 2%-5% according to the amount of magnesite powder and dolomite powder mixture. After mixing, the fixed carbon content of the raw ball is 1.8%-2.8%, and the magnesium-aluminum ratio of the ball is 0.8-0.

95. The wet overflow ball mill is fed according to the set value of the primary feed rate of 95-110t / h. The water supply is automatically calculated and added according to the slurry concentration to control the slurry concentration to 73%-76%. Steel balls are added to control the ball mill power to 2000-2600kwh, and the slurry mass fraction is between 73~76%. Ensure that the slurry particle size after ball milling is as follows: -200 mesh: 79~83%, -325 mesh: 60~68%, -400 mesh: 45~53%; Step 3: Ceramic dehydration: The slurry that meets the above particle size level is dehydrated by a ceramic filtration system, and the filter cake thickness is controlled at 12-15mm and the filter cake water content is controlled at 9.0-10.0%; Step 4: Mixing and pelletizing: In the secondary batching system, the dehydrated filter cake is mixed with fine powder return material and bentonite in proportion, mixed by a strong mixer, and then added to the drum pelletizing machine to produce green pellets. The diameter of the green pellets is controlled to be 8-16mm, the wet strength of the green pellets is controlled to be 1.0-1.5kg / ball, and the dry strength of the green pellets is controlled to be 5-10kg / ball; Step 5: Distribution and roasting: The raw pellets are operated through shuttle distribution belt conveyors and wide belt feeders to form a standardized material surface, that is, the material surface is flat, the thickness is uniform, the cross-section is a regular isosceles trapezoid, and there are no uneven structures such as pits, holes, and grooves on the material surface. The crushed granular material is then returned to the drum pelletizing machine through a roller distributor for re-pelletizing. Qualified raw pellets fall on the steel belt that has been laid with the base material, and enter the roasting furnace at a speed of 0.6-0.8m / min for drying, preheating, roasting and cooling to finally obtain finished pellets.

2. The method for producing high-magnesium flux chromium ore pellets according to claim 1, characterized in that: In the step 1, one or both of dolomite powder and magnesite powder can be added.

3. The method for producing high-magnesium flux chromium ore pellets according to claim 1, characterized in that: The material level of the intensive mixer in step 4 is controlled at 3.5-4.5t to ensure that the materials are evenly mixed in the intensive mixer and the moisture content of the materials is controlled between 10.0% and 10.8%.

4. The method for producing high-magnesium flux chromium ore pellets according to claim 1, characterized in that: In the step 4, 0-30 kg / t of fine powder return material, 11-13.5 kg / t of bentonite, and the moisture content of the raw pellets are 10.0-10.5%.

5. The method for producing high-magnesium flux chromium ore pellets according to claim 1, characterized in that: In step 5, the drying temperature is 380-500°C, and the air volume is the amount of air entering the furnace × (800-1000) Nm 3 / h, preheating temperature: 1050~1150℃, air volume: furnace volume × (450~550) Nm 3 / h, roasting section temperature: 1150~1250℃, air volume: furnace volume×(300~450)Nm 3 / h.