Method for comprehensively recovering selenium, mercury and lead from mercury-containing acid mud
Efficient recovery of selenium, mercury and lead from mercury-containing acid sludge through vacuum distillation-sulfation method, solving the problems of equipment corrosion and environmental pollution, and achieving efficient and clean metal recycling, with high yields and high levels of selenium, mercury and lead purity.
Patent Information
- Application Number
- CN202411136169.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing acid sludge treatment process has problems such as equipment corrosion, pollution of the environment and high cost, especially in the sulfurization and roasting method, the equipment has high corrosion resistance requirements, and the calcium-fixing selenium method and sodium carbonate smelting-reduction method are consumed more Reagent problems.
Using vacuum distillation-sulfation method, vacuum distillation is performed by drying mercury-containing acid sludge, mixing sulfur powder and then vacuum distillation is performed, and lead selenide, mercury sulfide and elemental selenium are gradually separated, and high-purity selenium, mercury and lead.
Efficient and clean recovery of selenium, mercury and lead from mercury-containing acid sludge is achieved. The selenium yield is greater than 99%, mercury is greater than 96%, and lead is greater than 90%, and the risks of equipment corrosion and environmental pollution are reduced.
Smart Images

Figure CN119020595A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of acid mud treatment metallurgy, in particular to a method for comprehensively recovering selenium, mercury and lead from mercury-containing acid mud. Background Art
[0002] During the high-temperature roasting process of lead-zinc concentrate, most of the volatile elements such as Hg, Se, and Pb in the minerals will evaporate into the flue gas. The gaseous mercury in the flue gas will react with other elements in the flue gas to form mercury-containing compounds. Before the flue gas enters the sulfuric acid workshop, these mercury-containing flue gases are generally collected in the dynamic wave scrubber of the purification process. After liquid-solid separation, acid sludge containing mercury, selenium, and lead is obtained. With the smelting production, the acid sludge produced by the factory is increasing, and the storage difficulty is increasing, which poses a certain threat to the surrounding environment and organisms. According to the provisions of international environmental protection treaties, mercury-containing acid sludge is identified as a hazardous waste.
[0003] At present, the acid sludge treatment process has the following problems: the wet selenium leaching and mercury solidification technology requires a relatively high pressure and has high requirements for equipment; in the calcium-added selenium solidification method, if the amount of air introduced during the CaO solidification selenium roasting process is insufficient, the oxidation degree of selenium may be insufficient, and HNO3 needs to be added subsequently to enhance the oxidation effect in order to allow selenium to be leached normally, which undoubtedly increases the process and subsequent costs; the sulfate roasting method requires the addition of concentrated sulfuric acid to the acid sludge for roasting, which is easy to corrode the equipment and has high requirements for the corrosion resistance of the equipment. There is also the problem of handling sulfur dioxide flue gas; the subsequent SO2 reduction process of the sodium carbonate smelting-reduction method requires the consumption of a large amount of hydrochloric acid and FeSO4 reagents. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies of the prior art, the present invention provides a method for comprehensively recovering selenium, mercury and lead from mercury-containing acid mud, thereby solving the problems of equipment corrosion and environmental pollution.
[0006] (II) Technical solution
[0007] To achieve the above object, the present invention is implemented by the following technical scheme: a method for comprehensively recovering selenium, mercury and lead from mercury-containing acid mud, comprising the following steps:
[0008] S1: drying the mercury-containing acid mud and then performing vacuum distillation to obtain lead selenide and mercury selenide condensate;
[0009] S2: uniformly mixing the condensate from step S1 with sulfur powder in a mixing bottle and then briquetting;
[0010] S3: vacuum distilling the mixture after briquetting in step S2 to obtain a mixture of lead sulfide, mercury sulfide and elemental selenium;
[0011] S4: vacuum distilling the mixture of step S3 to obtain a crude selenium condensate;
[0012] S5: vacuum distilling the residue of step S4 to obtain lead sulfide residue and mercuric sulfide condensate.
[0013] Preferably, the temperature rising procedure of the vacuum distillation includes: placing the required materials in a graphite crucible, placing the graphite crucible in a vacuum furnace, first turning on the circulating cooling water, then turning on the vacuum pump, and waiting for the vacuum degree to drop to 20-30Pa, starting the first temperature rising at a rate of 10-15°C / min; waiting for the first temperature rising to 200-250°C, heating up for the second time at a rate of 15-20°C / min; controlling the pressure in the furnace to be the target pressure, and heating up to the target temperature for the second time.
[0014] Preferably, the vacuum distillation in step S1 is carried out at a temperature of 700-800° C., for a time of 45-60 min, and at a vacuum degree of 1-10 Pa.
[0015] Preferably, the mixing ratio of the condensate and the sulfur powder in step S2 is 1:8.
[0016] Preferably, the vacuum distillation in step S3 is carried out at a temperature of 150 to 250° C., for a time of 20 to 30 min, and at a vacuum degree of 20 to 50 Pa.
[0017] Preferably, the vacuum distillation in step S4 is carried out at a temperature of 400 to 800° C., for a time of 30 to 60 min, and at a vacuum degree of 5 to 10 Pa.
[0018] Preferably, the vacuum distillation in step S5 is carried out at a temperature of 900-1000° C., for a time of 30-60 min, and at a vacuum degree of 1-10 Pa.
[0019] (III) Beneficial effects
[0020] The present invention provides a method for comprehensive recovery of selenium, mercury and lead from mercury-containing acid mud. The method has the following beneficial effects: the present invention adopts a vacuum distillation-sulfidation method, and the selenium yield is greater than 99%, the mercury is greater than 96%, the lead is greater than 90%, and the crude selenium purity is greater than 98%. The method realizes clean and efficient recovery of selenium, mercury and lead from mercury-containing acid mud. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1
[0024] The method for comprehensively recovering selenium, mercury and lead from mercury-containing acid mud has a process flow as follows: Figure 1 As shown, the specific steps are as follows: (1) 50g of dried mercury-containing acid mud is subjected to a vacuum distillation experiment under the conditions of 10Pa, 700°C and a heat preservation time of 45min to obtain a mixture of lead selenide and mercuric selenide (condensate); (2) the mixed condensate and sulfur powder are mixed in a mixing bottle at a ratio of 1:8, and then a vacuum distillation sulfidation experiment is carried out under the conditions of 250°C, 50Pa and a heat preservation time of 30min to obtain a mixture of lead sulfide, mercuric sulfide and elemental selenium; (3) the mixture is subjected to a vacuum distillation experiment under the conditions of 400°C, 10Pa and a heat preservation time of 30min to obtain a mixture of lead sulfide and mercuric sulfide (residue) and a crude selenium product (condensate); (4) the mixed residue is subjected to a vacuum distillation experiment under the conditions of 900°C, 10Pa and a heat preservation time of 30min to obtain lead sulfide (residue) and mercuric sulfide (condensate) products. Through analysis and detection, the selenium yield was 99.09%, the mercury yield was 96.83%, the lead yield was 90.91%, and the purity of the crude selenium product was 98.11%.
[0025] Example 2
[0026] The method for comprehensively recovering selenium, mercury and lead from mercury-containing acid mud has a process flow as follows: Figure 1As shown, the specific steps are as follows: (1) 50g of dried mercury-containing acid mud is subjected to a vacuum distillation experiment at 5Pa, 750°C, and a heat preservation time of 45min to obtain a mixture of lead selenide and mercuric selenide (condensate); (2) the mixed condensate and sulfur powder are mixed in a mixing bottle at a ratio of 1:8, and then a vacuum distillation sulfidation experiment is carried out at 200°C, 30Pa, and a heat preservation time of 25min to obtain a mixture of lead sulfide, mercuric sulfide and elemental selenium; (3) the mixture is subjected to a vacuum distillation experiment at 600°C, 8Pa, and a heat preservation time of 45min to obtain a mixture of lead sulfide and mercuric sulfide (residue) and a crude selenium product (condensate); (4) the mixed residue is subjected to a vacuum distillation experiment at 1000°C, 5Pa, and a heat preservation time of 45min to obtain lead sulfide (residue) and mercuric sulfide (condensate) products. Through analysis and detection, the selenium yield was 99.15%, the mercury yield was 97.04%, the lead yield was 91.30%, and the purity of the crude selenium product was 98.38%.
[0027] Example 3
[0028] The method for comprehensively recovering selenium, mercury and lead from mercury-containing acid mud has a process flow as follows: Figure 1 As shown, the specific steps are as follows: (1) 100g of dried mercury-containing acid mud is subjected to a vacuum distillation experiment under the conditions of 1Pa, 800°C and a heat preservation time of 60min to obtain a mixture of lead selenide and mercuric selenide (condensate); (2) the mixed condensate and sulfur powder are mixed in a mixing bottle at a ratio of 1:8, and then a vacuum distillation sulfidation experiment is carried out under the conditions of 150°C, 20Pa and a heat preservation time of 20min to obtain a mixture of lead sulfide, mercuric sulfide and elemental selenium; (3) the mixture is subjected to a vacuum distillation experiment under the conditions of 800°C, 5Pa and a heat preservation time of 60min to obtain a mixture of lead sulfide and mercuric sulfide (residue) and a crude selenium product (condensate); (4) the mixed residue is subjected to a vacuum distillation experiment under the conditions of 1100°C, 1Pa and a heat preservation time of 60min to obtain lead sulfide (residue) and mercuric sulfide (condensate) products. Through analysis and detection, the selenium yield was 99.51%, the mercury yield was 97.82%, the lead yield was 91.46%, and the purity of the crude selenium product was 99.12%.
[0029] Based on the above examples 1-3, the vacuum distillation-sulfidation method used in the present invention for treating mercury-containing acid mud has a selenium yield greater than 99%, mercury greater than 96%, and lead greater than 90%, and the purity of the obtained crude selenium product is greater than 98%. The process flow of this design is simple, the mercury enrichment effect is good, the selenium recovery rate is high, it is clean and pollution-free, and has broad application prospects.
[0030] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for comprehensive recovery of selenium, mercury and lead from mercury-containing acid mud, characterized in that: The following steps are involved: S1: drying the mercury-containing acid mud and then performing vacuum distillation to obtain lead selenide and mercury selenide condensate; S2: uniformly mixing the condensate from step S1 with sulfur powder in a mixing bottle and then briquetting; S3: vacuum distilling the mixture after briquetting in step S2 to obtain a mixture of lead sulfide, mercury sulfide and elemental selenium; S4: vacuum distilling the mixture of step S3 to obtain a crude selenium condensate; S5: vacuum distilling the residue of step S4 to obtain lead sulfide residue and mercuric sulfide condensate.
2. The method for comprehensive recovery of selenium, mercury and lead from mercury-containing acid mud according to claim 1, characterized in that: The temperature rising procedure of the vacuum distillation comprises: placing the required materials in a graphite crucible, placing the graphite crucible in a vacuum furnace, first turning on the circulating cooling water, then turning on the vacuum pump, and starting the first temperature rising after the vacuum degree drops to 20-30 Pa, with a temperature rising rate of 10-15° C. / min; after the first temperature rising to 200-250° C., performing the second temperature rising at a temperature rising rate of 15-20° C. / min; controlling the pressure in the furnace to be the target pressure, and heating to the target temperature for the second time.
3. The method for comprehensive recovery of selenium, mercury and lead from mercury-containing acid mud according to claim 1, characterized in that: The vacuum distillation temperature of step S1 is 700-800° C., the time is 45-60 min, and the vacuum degree is 1-10 Pa.
4. The method for comprehensive recovery of selenium, mercury and lead from mercury-containing acid mud according to claim 1, characterized in that: The mixing ratio of the condensate and the sulfur powder in step S2 is 1:
8.
5. The method for comprehensive recovery of selenium, mercury and lead from mercury-containing acid mud according to claim 1, characterized in that: The temperature of the vacuum distillation in step S3 is 150-250° C., the time is 20-30 min, and the vacuum degree is 20-50 Pa.
6. The method for comprehensive recovery of selenium, mercury and lead from mercury-containing acid mud according to claim 1, characterized in that: The vacuum distillation temperature of step S4 is 400-800° C., the time is 30-60 min, and the vacuum degree is 5-10 Pa.
7. The method for comprehensive recovery of selenium, mercury and lead from mercury-containing acid mud according to claim 1, characterized in that: The temperature of the vacuum distillation in step S5 is 900-1000° C., the time is 30-60 min, and the vacuum degree is 1-10 Pa.
Citation Information
Cited By
Method and system for synergistically recovering mercury and selenium from acid mud based on Fe (III) / Fe (II)-O2 catalytic circulation and selective oxidation coupling
CN122303598A