Method for extracting chromium from chromium-containing material through liquid-phase oxidation

By using additives of Cr, Fe, Si, C and other elements in the liquid phase oxidation process of chromite ore for low-temperature roasting treatment, the problems of high reaction temperature and impurity content in the prior art are solved, and the efficiency of chromium is achieved Extraction and resource utilization reduce production costs.

CN119020616AActive Publication Date: 2024-11-26HUBEI ZHENHUA CHEMICAL CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411118936.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The existing liquid-phase oxidation method of chromium iron ore has high reaction temperature, serious equipment corrosion, high impurity content of products, and complex tailings, resulting in low chromium resource utilization and high production costs.

Method used

The chromium-containing materials are subjected to low-temperature roasting with specific additives (Cr, Fe, Si, C) to improve the liquid phase oxidation reaction rate, reduce the reaction temperature and time, and generate highly oxidized ferrate and sodium aluminosilicate through alkaline roasting. Precipitation to reduce impurity content.

Benefits of technology

The efficient extraction of chromium was achieved, the chromium conversion rate reached more than 96%, and the chromium content in the tailings was less than 1.2%, reducing production costs and energy consumption, and promoting the resource utilization of ferrochromium alloys and slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004994452470000131
    Figure BDA0004994452470000131
Patent Text Reader

Abstract

The invention provides a method for extracting chromium from a chromium-containing material through liquid-phase oxidation, which comprises the following steps: (1) mixing the chromium-containing material, alkali and an additive, and roasting to obtain roasted clinker; the additive comprises the following elements: Cr, Fe, Si and C; (2) mixing a solvent with the roasted clinker in the step (1), heating, introducing oxidizing gas, and reacting to obtain mixed slurry; according to the method, the specific additive is added, and the chromium-containing material is subjected to low-temperature roasting treatment, so that the reaction rate of liquid-phase oxidation chromium extraction can be obviously increased, the conversion rate of chromium is increased, the reaction temperature of liquid-phase oxidation is reduced, the reaction time of liquid-phase oxidation is shortened, the chromium content in the tailings is reduced, meanwhile, resource utilization of the ferrochrome and the tailings is achieved, and the method is suitable for industrial production. The production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chromium salt production and waste residue utilization, and relates to a method for extracting chromium by liquid-phase oxidation of chromium-containing materials. Background Art

[0002] As an important strategic metal resource, chromium is widely used in the fields of steel, metallurgy, chemical industry, medicine, aerospace, etc. In recent years, with the continuous development of the economy, the demand for chromium resources has also increased. Chromite, as the most valuable chromium-containing mineral, is the main raw material for the production of chromium and chromium salts. In the production process of chromium salts, the utilization rate of chromium resources is low, and the hexavalent chromium produced is extremely harmful to the human body and the environment. Therefore, making full use of the chromium in chromite and solving the pollution problem in its production process have become urgent issues to be solved.

[0003] In recent years, various processes for liquid phase oxidation of chromite have been developed based on the characteristics of raw materials for the utilization of chromium-containing minerals such as chromite and the production of chromium salts. CN1226512A discloses a clean production method for sodium chromate, which includes oxidative decomposition of chromite in a NaOH molten salt medium, a reaction temperature of 500-550°C, and leaching the product in a high alkalinity area; the hexavalent chromium leachate is cooled and crystallized simultaneously to obtain a mixed type of sodium chromate and sodium aluminate coarse crystals and a crystallization mother liquor, the coarse crystals are countercurrently washed and purified to obtain a purified sodium chromate crystal product and a coarse crystal washing liquid, and the coarse crystal washing liquid is alkali adjusted and crystallized to separate sodium aluminate. However, the reaction temperature of this method is high, and the high-concentration leachate is directly cooled and crystallized, the solution viscosity is large, and solid-liquid separation is difficult. In addition, the equipment is severely corroded in a high temperature and high alkaline environment; the mixed crystals need to be further separated, and the industrial process is long.

[0004] CN101481144A discloses a clean production method for preparing potassium chromate from chromite, wherein the chromite is oxidized and decomposed with an oxidant in a KOH-KNO3-H2O medium at a certain temperature, at which temperature KNO3 is not an oxidant but a reaction medium and can be recycled, and the oxidant is oxygen, a gas with a certain oxygen partial pressure or a peroxide. However, the production process of this method is long.

[0005] CN109399716A discloses a method for extracting chromium from chromium-containing materials by liquid-phase oxidation. The method comprises the steps of extracting chromium by liquid-phase oxidation using chromium-containing materials and alkali as raw materials, wherein the raw materials also include additives, wherein the additives include transition metal compounds, and the additives are selected from black slag and / or chromium-containing waste catalysts, wherein the black slag is chromium slag having a Cr2O3 content higher than 15wt% obtained by sorting leached slag from liquid-phase oxidation for chromium extraction; the method introduces transition metal compounds for the purpose of improving the conversion rate of chromium in the chromium-containing materials, but this will result in a high impurity content in the product and a complex tailings composition.

[0006] In summary, for the method of extracting chromium by liquid-phase oxidation of chromium-containing materials, it is also necessary to develop a new type of additive and a pretreatment method for chromium-containing materials to strengthen the liquid-phase oxidation process, improve the conversion rate of chromium in the liquid-phase oxidation process of chromium-containing materials, reduce temperature and pressure, and at the same time reduce the content of impurities such as silicon and aluminum in the leaching solution, reduce waste slag emissions, thereby reducing energy consumption and production costs. Summary of the invention

[0007] The object of the present invention is to provide a method for extracting chromium by liquid phase oxidation of chromium-containing materials. By adding specific additives and performing low-temperature roasting treatment on the chromium-containing materials, the reaction rate of liquid phase oxidation to extract chromium can be significantly accelerated, the conversion rate of chromium can be improved, the reaction temperature of liquid phase oxidation can be reduced, the reaction time of liquid phase oxidation can be shortened, the chromium content in tailings can be reduced, and at the same time, the resource utilization of ferrochrome alloy and slag can be realized, and the production cost can be reduced.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for extracting chromium by liquid-phase oxidation of chromium-containing materials, the method comprising the following steps:

[0010] (1) mixing a chromium-containing material, an alkali and an additive and then roasting the mixture to obtain a roasted clinker;

[0011] The additives include the following elements: Cr, Fe, Si, C;

[0012] (2) The solvent and the calcined clinker obtained in step (1) are mixed and heated, and an oxidizing gas is introduced to obtain a mixed slurry after reaction.

[0013] The method for extracting chromium by liquid-phase oxidation of chromium-containing materials provided by the present invention can significantly accelerate the reaction rate of liquid-phase oxidation to extract chromium, improve the conversion rate of chromium, reduce the reaction temperature of liquid-phase oxidation, shorten the reaction time of liquid-phase oxidation, reduce the chromium content in tailings, and realize resource utilization of chromium in the additive, reduce production costs, and have good economic benefits by adding specific additives and performing low-temperature roasting pretreatment on the mixed materials.

[0014] It is worth noting that the additive used in the present invention has the following functions: first, it can realize the resource utilization of chromium in the additive and reduce the existing storage volume of waste slag; second, the iron element in the additive is more likely to generate ferrate with higher oxidizability, which helps to destroy the internal structure of the chromium-containing material during the liquid phase oxidation process and realize low-temperature and low-pressure leaching; third, the carbon in the additive has a higher calorific value, which can achieve a better activation effect on the chromium-containing material at a lower temperature, and at the same time helps to increase the porosity of the material, thereby improving the transportation efficiency of the oxygen-containing gas and realizing the efficient extraction of chromium during the liquid phase oxidation chromium extraction process; fourth, the silicon in the additive generates sodium aluminosilicate precipitate with aluminum in the chromite under alkaline roasting conditions, thereby reducing the impurity aluminum content in the solution.

[0015] As a preferred technical solution of the present invention, the chromium-containing material in step (1) includes chromite and / or chromium slag.

[0016] In the present invention, the chromite ore and chromium slag both contain a certain content of Cr2O3.

[0017] Preferably, the average particle size of the chromium-containing material in step (1) is ≤74 μm, for example, it can be 72 μm, 70 μm, 68 μm, 65 μm, 60 μm, 55 μm, 50 μm or 40 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] As a preferred technical solution of the present invention, the alkali in step (1) includes sodium hydroxide and / or potassium hydroxide, preferably sodium hydroxide.

[0019] Preferably, the amount of alkali added in step (1) is 0.5 to 3 times the mass of the alkali consumed when all chromium in the chromium-containing material and additive is converted into sodium chromate, for example, it can be 0.6 times, 0.8 times, 1 times, 1.2 times, 1.5 times, 1.8 times, 2 times, 2.2 times, 2.5 times or 2.8 times, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] In the present invention, the amount of alkali added is the theoretical consumption.

[0021] As a preferred technical solution of the present invention, the additive in step (1) includes the following elements in terms of mass content: Cr: 30wt.%~60wt.%, Fe: 10wt.%~30wt.%, Si: 1wt.%~20wt.%, C: 5wt.%~30wt.%, and the remainder is O and unavoidable impurities.

[0022] In the present invention, the additive contains 30wt.% to 60wt.% of Cr element, for example, 32wt.%, 35wt.%, 38wt.%, 40wt.%, 42wt.%, 45wt.%, 48wt.%, 50wt.%, 52wt.%, 55wt.% or 58wt.%, etc., and the additive contains 10wt.% to 30wt.% of Fe element, for example, 12wt.%, 15wt.%, 18wt.%, 20wt.%, 22wt.%, 25wt.% or 28wt.%, etc. The additive contains 1wt.% to 20wt.% of Si element, for example, 2wt.%, 5wt.%, 8wt.%, 10wt.%, 12wt.%, 15wt.% or 18wt.%, etc. The additive contains 5wt.% to 30wt.% of C element, for example, 8wt.%, 10wt.%, 12wt.%, 15wt.%, 18wt.%, 20wt.%, 22wt.%, 25wt.% or 28wt.%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0023] Preferably, the additive in step (1) includes the following elements by mass content: Cr: 30wt.%~55wt.%, Fe: 10wt.%~30wt.%, Si: 5wt.%~20wt.%, C: 5wt.%~24wt.%, and the remainder is O and unavoidable impurities.

[0024] Preferably, the additive in step (1) comprises any one of ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue, or a combination of at least two of them, wherein the combinations are typically but not limitatively: a combination of ferrochrome and ferrochrome acid leaching residue, a combination of ferrochrome acid leaching residue and ferrochrome chlorination decomposition residue, or a combination of ferrochrome, ferrochrome acid leaching residue and ferrochrome chlorination decomposition residue, etc.

[0025] In the present invention, ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue is selected as an additive, so that chromium in the ferrochrome or its leaching residue can be fully extracted, and the reaction rate and conversion rate of chromium extraction by liquid phase oxidation are improved, the reaction temperature of liquid phase oxidation is reduced, and the reaction time of liquid phase oxidation is shortened.

[0026] Preferably, the mass ratio of the additive to the chromium-containing material in step (1) is (0.2-3):1, for example, it can be 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 2:1, 2.2:1, 2.4:1, 2.5:1, 2.6:1, 2.8:1 or 2.9:1, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably (0.5-2):1.

[0027] Preferably, the average particle size of the additive in step (1) is ≤74 μm, for example, it can be 72 μm, 70 μm, 68 μm, 65 μm, 60 μm, 55 μm, 50 μm or 40 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] As a preferred technical solution of the present invention, the calcination temperature in step (1) is 100-500°C, for example, it can be 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C or 480°C, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 200-400°C.

[0029] Preferably, the calcination time in step (1) is 10 to 180 min, for example, it can be 20 min, 30 min, 40 min, 50 min, 60 min, 80 min, 100 min, 110 min, 120 min, 140 min, 150 min, 160 min or 180 min, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 30 to 120 min.

[0030] Preferably, the calcination in step (1) is carried out in air and / or oxygen-rich gas.

[0031] In the present invention, the oxygen-rich gas is an atmosphere in which the volume percentage of oxygen is greater than 20%.

[0032] As a preferred technical solution of the present invention, the solvent in step (2) includes water.

[0033] Preferably, the liquid-to-solid ratio of the solvent to the roasted clinker in step (2) is (2-15):1 mL / g, for example, it can be 3:1 mL / g, 4:1 mL / g, 5:1 mL / g, 6:1 mL / g, 7:1 mL / g, 8:1 mL / g, 9:1 mL / g, 10:1 mL / g, 12:1 mL / g or 14:1 mL / g, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably (4-10):1 mL / g.

[0034] As a preferred technical solution of the present invention, the heating temperature in step (2) is 100-250°C, for example, it can be 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 180°C, 200°C, 220°C or 240°C, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 120-200°C.

[0035] Preferably, the heating time in step (2) is 0.5 to 5 h, for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h or 4.5 h, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 1 to 4 h.

[0036] As a preferred technical solution of the present invention, the oxidizing gas in step (2) includes air and / or oxygen, preferably oxygen.

[0037] Preferably, the oxidizing gas in step (2) is introduced continuously.

[0038] Preferably, the oxygen partial pressure during the heating process of step (2) is 0.2 to 6 MPa, for example, it can be 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, 3.5 MPa, 4 MPa or 4.5 MPa, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 1 to 4 MPa.

[0039] As a preferred technical solution of the present invention, the method further comprises: performing solid-liquid separation on the mixed slurry in step (2) to obtain chromium-containing alkali solution and tailings.

[0040] As a preferred technical solution of the present invention, the method comprises the following steps:

[0041] (1) mixing a chromium-containing material, an alkali and an additive, and roasting them in air and / or oxygen-rich gas at a temperature of 100 to 500° C. for 10 to 180 minutes to obtain a roasted clinker;

[0042] The chromium-containing material comprises chromite and / or chromium slag; the alkali comprises sodium hydroxide and / or potassium hydroxide; the additive comprises the following elements according to mass content: Cr: 30wt.%-60wt.%, Fe: 10wt.%-30wt.%, Si: 1wt.%-20wt.%, C: 5wt.%-30wt.%, the remainder being O and unavoidable impurities; the additive comprises any one of ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue or a combination of at least two thereof; the amount of the alkali added is 0.5-3 times the mass of the alkali consumed when all chromium in the chromium-containing material and the additive is converted into sodium chromate; the mass ratio of the additive to the chromium-containing material is (0.2-3):1;

[0043] (2) mixing the solvent and the calcined clinker of step (1) at a liquid-to-solid ratio of (2-15):1 mL / g, heating at a temperature of 100-250° C. for 0.5-5 h, and continuously introducing an oxidizing gas until the oxygen partial pressure is 0.2-6 MPa, obtaining a mixed slurry after the reaction, and then performing solid-liquid separation to obtain a chromium-containing alkali solution and tailings;

[0044] The oxidizing gas includes air and / or oxygen.

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] The method for extracting chromium by liquid-phase oxidation of chromium-containing materials provided by the present invention can significantly accelerate the reaction rate of extracting chromium by liquid-phase oxidation, improve the conversion rate of chromium, reduce the reaction temperature of liquid-phase oxidation, shorten the reaction time of liquid-phase oxidation, reduce the chromium content in tailings, and realize resource utilization of chromium in the additive, reduce production costs, and have good economic benefits. The conversion rate of chromium can reach more than 96%, and the chromium content in the tailings is less than 1.2%. DETAILED DESCRIPTION

[0047] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0048] In the following examples and comparative examples, the oxygen-rich gas is a gas having an oxygen content greater than 20% by volume.

[0049] Example 1

[0050] This embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, the method comprising the following steps:

[0051] (1) mixing chromite, sodium hydroxide and chromium iron acid leaching residue, wherein the average particle size of the mixture is less than 50 μm, and roasting the mixture in an air atmosphere at a temperature of 350° C. for 60 minutes to obtain roasted clinker;

[0052] The content of Cr2O3 in the chromite is 43wt.%; the ferrochrome acid leaching residue includes the following elements by mass content: Cr: 40wt.%, Fe: 25wt.%, Si: 9wt.%, C: 13wt.%, and the remainder is O and unavoidable impurities; the amount of sodium hydroxide added is twice the mass of the alkali consumed when all chromium in the chromite and the ferrochrome acid leaching residue is converted into sodium chromate; the mass ratio of the ferrochrome acid leaching residue to the chromite is 0.8:1;

[0053] (2) Deionized water and the calcined clinker of step (1) are stirred and mixed at a liquid-to-solid ratio of 8:1 mL / g, heated to a temperature of 150° C., oxygen is continuously introduced until the oxygen partial pressure reaches 3 MPa, and this pressure is maintained for a reaction of 2 h to obtain a mixed slurry, and then the mixed slurry is subjected to solid-liquid separation to obtain a chromium-containing alkali solution and tailings.

[0054] Example 2

[0055] This embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, the method comprising the following steps:

[0056] (1) mixing chromium slag, sodium hydroxide and ferrochrome, wherein the average particle size of the mixture is less than 45 μm, and roasting the mixture in an air atmosphere at a temperature of 300° C. for 90 minutes to obtain roasted clinker;

[0057] The content of Cr2O3 in the chromium slag is 9wt.%; the ferrochrome includes the following elements by mass content: Cr: 53wt.%, Fe: 25wt.%, Si: 10wt.%, C: 6.2wt.%, and the remainder is O and unavoidable impurities; the amount of sodium hydroxide added is 1.5 times the mass of the alkali consumed when all the chromium in the chromium slag and ferrochrome is converted into sodium chromate; the mass ratio of the ferrochrome to the chromium slag is 1:1;

[0058] (2) Deionized water and the calcined clinker of step (1) are stirred and mixed at a liquid-to-solid ratio of 10:1 mL / g, heated to a temperature of 180° C., oxygen is continuously introduced until the oxygen partial pressure reaches 3.5 MPa, and this pressure is maintained for a reaction of 3 hours to obtain a mixed slurry, and then the mixed slurry is subjected to solid-liquid separation to obtain a chromium-containing alkali solution and tailings.

[0059] Example 3

[0060] This embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, the method comprising the following steps:

[0061] (1) mixing chromite, sodium hydroxide and ferrochrome acid leaching residue, wherein the average particle size of the mixture is less than 55 μm, and roasting the mixture in an air atmosphere at a temperature of 250° C. for 120 minutes to obtain roasted clinker;

[0062] The content of Cr2O3 in the chromite is 43wt.%; the ferrochrome acid leaching residue includes the following elements by mass content: Cr: 36wt.%, Fe: 19wt.%, Si: 17wt.%, C: 15wt.%, and the remainder is O and unavoidable impurities; the amount of sodium hydroxide added is 1.8 times the mass of the alkali consumed by converting all the chromium in the chromite and the ferrochrome acid leaching residue into sodium chromate; the mass ratio of the ferrochrome acid leaching residue to the chromite is 0.5:1;

[0063] (2) Deionized water and the calcined clinker of step (1) are stirred and mixed at a liquid-to-solid ratio of 5:1 mL / g, heated to a temperature of 200° C., oxygen is continuously introduced until the oxygen partial pressure reaches 2.5 MPa, and this pressure is maintained for a reaction of 2 h to obtain a mixed slurry, and then the mixed slurry is subjected to solid-liquid separation to obtain a chromium-containing alkali solution and tailings.

[0064] Example 4

[0065] This embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, the method comprising the following steps:

[0066] (1) mixing chromium slag, sodium hydroxide and ferrochrome acid leaching residue, wherein the average particle size of the mixture is less than 65 μm, and roasting the mixture in an oxygen-rich gas at a temperature of 320° C. for 100 minutes to obtain roasted clinker;

[0067] The content of Cr2O3 in the chromium slag is 9wt.%; the ferrochrome acid leaching slag includes the following elements by mass content: Cr: 45wt.%, Fe: 29wt.%, Si: 8wt.%, C: 9wt.%, and the remainder is O and unavoidable impurities; the amount of sodium hydroxide added is 2.8 times the mass of alkali consumed by converting all chromium in the chromium slag and ferrochrome acid leaching slag into sodium chromate; the mass ratio of the ferrochrome acid leaching slag to the chromium slag is 0.9:1;

[0068] (2) Deionized water and the calcined clinker of step (1) are stirred and mixed at a liquid-to-solid ratio of 7:1 mL / g, heated to a temperature of 180° C., oxygen is continuously introduced until the oxygen partial pressure reaches 3.6 MPa, and this pressure is maintained for a reaction of 3.5 hours to obtain a mixed slurry, and then the mixed slurry is subjected to solid-liquid separation to obtain a chromium-containing alkali solution and tailings.

[0069] Example 5

[0070] This embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, the method comprising the following steps:

[0071] (1) mixing chromite, sodium hydroxide and chromium iron chlorination decomposition slag, wherein the average particle size of the mixture is less than 35 μm, and roasting the mixture in an oxygen-rich atmosphere at a temperature of 350° C. for 60 minutes to obtain roasted clinker;

[0072] The content of Cr2O3 in the chromite is 43wt.%; the ferrochrome chlorination decomposition slag includes the following elements by mass content: Cr: 38wt.%, Fe: 17wt.%, Si: 16wt.%, C: 21wt.%, and the remainder is O and unavoidable impurities; the amount of sodium hydroxide added is 1.8 times the mass of the alkali consumed when all chromium in the chromite and the ferrochrome chlorination decomposition slag is converted into sodium chromate; the mass ratio of the ferrochrome chlorination decomposition slag to the chromite is 1.5:1;

[0073] (2) Deionized water and the calcined clinker of step (1) are stirred and mixed at a liquid-to-solid ratio of 4:1 mL / g, heated to a temperature of 120° C., oxygen is continuously introduced until the oxygen partial pressure reaches 4 MPa, and this pressure is maintained for a reaction of 3 hours to obtain a mixed slurry, and then the mixed slurry is subjected to solid-liquid separation to obtain a chromium-containing alkali solution and tailings.

[0074] Example 6

[0075] This embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, the method comprising the following steps:

[0076] (1) mixing chromium slag, sodium hydroxide and chromium iron chlorination decomposition slag, wherein the average particle size of the mixture is less than 45 μm, and roasting the mixture in an oxygen-rich atmosphere at a temperature of 250° C. for 120 minutes to obtain roasted clinker;

[0077] The content of Cr2O3 in the chromium slag is 9wt.%; the ferrochrome chlorination decomposition slag includes the following elements by mass content: Cr: 50wt.%, Fe: 20wt.%, Si: 10wt.%, C: 8wt.%, and the remainder is O and unavoidable impurities; the amount of sodium hydroxide added is 2.6 times the mass of the alkali consumed when all chromium in the chromium slag and the ferrochrome chlorination decomposition slag is converted into sodium chromate; the mass ratio of the ferrochrome chlorination decomposition slag to the chromium slag is 0.5:1;

[0078] (2) Deionized water and the calcined clinker of step (1) are stirred and mixed at a liquid-to-solid ratio of 9:1 mL / g, heated to a temperature of 150° C., oxygen is continuously introduced until the oxygen partial pressure reaches 3.4 MPa, and this pressure is maintained for a reaction of 3 hours to obtain a mixed slurry, and then the mixed slurry is subjected to solid-liquid separation to obtain a chromium-containing alkali solution and tailings.

[0079] Example 7

[0080] This embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, the method comprising the following steps:

[0081] (1) mixing chromite, sodium hydroxide and chromium iron acid leaching residue, wherein the average particle size of the mixture is less than 38 μm, and roasting the mixture in an air atmosphere at a temperature of 400° C. for 120 minutes to obtain roasted clinker;

[0082] The content of Cr2O3 in the chromite is 43wt.%; the ferrochrome acid leaching residue includes the following elements by mass content: Cr: 31wt.%, Fe: 12wt.%, Si: 13wt.%, C: 11wt.%, and the remainder is O and unavoidable impurities; the amount of sodium hydroxide added is 2.5 times the mass of alkali consumed by converting all chromium in the chromite and ferrochrome acid leaching residue into sodium chromate; the mass ratio of the ferrochrome acid leaching residue to the chromite is 1.8:1;

[0083] (2) deionized water and the calcined clinker of step (1) are stirred and mixed at a liquid-to-solid ratio of 8:1 mL / g, heated to a temperature of 200° C., oxygen is continuously introduced until the oxygen partial pressure reaches 4 MPa, and this pressure is maintained for a reaction of 4 hours to obtain a mixed slurry, and then the mixed slurry is subjected to solid-liquid separation to obtain a chromium-containing alkali solution and tailings.

[0084] Example 8

[0085] This embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, the method comprising the following steps:

[0086] (1) mixing chromium slag, sodium hydroxide and ferrochrome acid leaching residue, wherein the average particle size of the mixture is less than 74 μm, and roasting the mixture in an air atmosphere at a temperature of 250° C. for 60 minutes to obtain roasted clinker;

[0087] The content of Cr2O3 in the chromium slag is 9wt.%; the ferrochrome acid leaching slag includes the following elements by mass content: Cr: 32wt.%, Fe: 27wt.%, Si: 12wt.%, C: 10wt.%, and the remainder is O and unavoidable impurities; the amount of sodium hydroxide added is 3 times the mass of alkali consumed by converting all chromium in the chromium slag and ferrochrome acid leaching slag into sodium chromate; the mass ratio of the ferrochrome acid leaching slag to the chromium slag is 2:1;

[0088] (2) Deionized water and the calcined clinker of step (1) are stirred and mixed at a liquid-to-solid ratio of 5:1 mL / g, heated to a temperature of 120° C., oxygen is continuously introduced until the oxygen partial pressure reaches 3 MPa, and this pressure is maintained for a reaction of 4 hours to obtain a mixed slurry, and then the mixed slurry is subjected to solid-liquid separation to obtain a chromium-containing alkali solution and tailings.

[0089] Example 9

[0090] The present embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, except that the ferrochrome acid leaching residue in step (1) comprises the following elements by mass content: Cr: 40wt.%, Fe: 5wt.%, Si: 9wt.%, C: 13wt.%, and the remainder is O and unavoidable impurities; other conditions are the same as those in Example 1.

[0091] Example 10

[0092] The present embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, except that the ferrochrome acid leaching residue in step (1) comprises the following elements by mass content: Cr: 40wt.%, Fe: 25wt.%, Si: 9wt.%, C: 2wt.%, and the remainder is O and unavoidable impurities; other conditions are the same as those in Example 1.

[0093] Embodiment 11

[0094] This embodiment provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation, except that the mass ratio of the ferrochromium acid leaching residue to the chromite ore in step (1) is 3.5:1; other conditions are the same as those in Example 1.

[0095] Comparative Example 1

[0096] This comparative example provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation. Except that no ferrochromium acid leaching residue is added in step (1), other conditions are the same as those in Example 1.

[0097] Comparative Example 2

[0098] This comparative example provides a method for extracting chromium from a chromium-containing material by liquid phase oxidation. Except that roasting is not performed in step (1), other conditions are the same as those in Example 1.

[0099] The conversion rate of chromium in the chromium-containing alkali solution obtained in step (2) of the above embodiment and comparative example and the chromium content in the tailings were tested respectively, wherein the chromium content (in terms of Cr2O3) was detected by ICP. The results are shown in Table 1.

[0100] Table 1

[0101]

[0102] From Table 1, we can see that:

[0103] (1) The method for extracting chromium from chromium-containing materials by liquid phase oxidation provided in Examples 1-8 of the present invention can significantly accelerate the reaction rate of chromium extraction by liquid phase oxidation, improve the conversion rate of chromium, reduce the reaction temperature of liquid phase oxidation, shorten the reaction time of liquid phase oxidation, and reduce the chromium content in the tailings by adding specific additives and pre-treating the mixed materials with low temperature roasting; wherein the conversion rate of chromium is greater than 96%, and the chromium content in the tailings is less than 1.2%;

[0104] (2) From the comparison between Example 1 and Examples 9-10, it can be seen that when the Fe content in the additive is low, it is not conducive to the leaching of chromium in the chromium-containing material during the liquid phase oxidation process; when the C content in the additive is low, it is not conducive to improving the porosity of the material, and thus the transport efficiency of the oxygen-containing gas cannot be improved, resulting in a slight decrease in the conversion rate of chromium;

[0105] (3) It can be seen from the comparison between Example 1 and Example 11 that when the amount of additives used is too much, due to the large amount of additives added, some additives cannot play a role, the chromium extraction rate is not further improved, and the chromium content in the slag is increased;

[0106] (4) By comparing Example 1 with Comparative Examples 1-2, it can be seen that when no additive is added or the mixed material is not subjected to low-temperature calcination treatment, the reaction rate of liquid-phase oxidation chromium extraction will be prolonged, which is not conducive to the efficient extraction and recovery of chromium from the chromium-containing material, resulting in a decrease in the conversion rate of chromium and an increase in the chromium content in the tailings.

[0107] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for extracting chromium from chromium-containing materials by liquid phase oxidation, characterized in that: The method comprises the following steps: (1) mixing a chromium-containing material, an alkali and an additive and then roasting the mixture to obtain a roasted clinker; The additives include the following elements: Cr, Fe, Si, C; (2) The solvent and the calcined clinker obtained in step (1) are mixed and heated, and an oxidizing gas is introduced to obtain a mixed slurry after reaction.

2. The method according to claim 1, characterized in that The chromium-containing material in step (1) includes chromite and / or chromium slag; Preferably, the average particle size of the chromium-containing material in step (1) is ≤74 μm.

3. The method according to claim 1 or 2, characterized in that: The alkali in step (1) comprises sodium hydroxide and / or potassium hydroxide, preferably sodium hydroxide; Preferably, the amount of alkali added in step (1) is 0.5 to 3 times the mass of the alkali consumed when all chromium in the chromium-containing material and additive is converted into sodium chromate.

4. The method according to any one of claims 1 to 3, characterized in that: The additive in step (1) comprises the following elements by mass content: Cr: 30wt.% to 60wt.%, Fe: 10wt.% to 30wt.%, Si: 1wt.% to 20wt.%, C: 5wt.% to 30wt.%, and the remainder is O and unavoidable impurities; Preferably, the additive in step (1) comprises the following elements by mass content: Cr: 30wt.% to 55wt.%, Fe: 10wt.% to 30wt.%, Si: 5wt.% to 20wt.%, C: 5wt.% to 24wt.%, and the remainder is O and unavoidable impurities; Preferably, the additive in step (1) comprises any one of ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue, or a combination of at least two thereof; Preferably, the mass ratio of the additive to the chromium-containing material in step (1) is (0.2-3):1, preferably (0.5-2):1; Preferably, the average particle size of the additive in step (1) is ≤74 μm.

5. The method according to any one of claims 1 to 4, characterized in that: The calcination temperature in step (1) is 100-500° C., preferably 200-400° C.; Preferably, the calcination time in step (1) is 10 to 180 min, preferably 30 to 120 min; Preferably, the calcination in step (1) is carried out in air and / or oxygen-rich gas.

6. The method according to any one of claims 1 to 5, characterized in that: The solvent in step (2) includes water; Preferably, the liquid-to-solid ratio of the solvent to the roasted clinker in step (2) is (2-15):1 mL / g, preferably (4-10):1 mL / g.

7. The method according to any one of claims 1 to 6, characterized in that: The heating temperature in step (2) is 100 to 250° C., preferably 120 to 200° C.; Preferably, the heating time in step (2) is 0.5 to 5 hours, preferably 1 to 4 hours.

8. The method according to any one of claims 1 to 7, characterized in that: The oxidizing gas in step (2) includes air and / or oxygen, preferably oxygen; Preferably, the oxidizing gas in step (2) is introduced continuously; Preferably, the oxygen partial pressure during the heating process in step (2) is 0.2 to 6 MPa, preferably 1 to 4 MPa.

9. The method according to any one of claims 1 to 8, characterized in that: The method further comprises: performing solid-liquid separation on the mixed slurry in step (2) to obtain chromium-containing alkali solution and tailings.

10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) mixing a chromium-containing material, an alkali and an additive, and roasting them in air and / or oxygen-rich gas at a temperature of 100 to 500° C. for 10 to 180 minutes to obtain a roasted clinker; The chromium-containing material comprises chromite and / or chromium slag; the alkali comprises sodium hydroxide and / or potassium hydroxide; the additive comprises the following elements according to mass content: Cr: 30wt.%-60wt.%, Fe: 10wt.%-30wt.%, Si: 1wt.%-20wt.%, C: 5wt.%-30wt.%, the remainder being O and unavoidable impurities; the additive comprises any one of ferrochrome, ferrochrome acid leaching residue or ferrochrome chlorination decomposition residue or a combination of at least two thereof; the amount of the alkali added is 0.5-3 times the mass of the alkali consumed when all chromium in the chromium-containing material and the additive is converted into sodium chromate; the mass ratio of the additive to the chromium-containing material is (0.2-3):1; (2) mixing the solvent and the calcined clinker of step (1) at a liquid-to-solid ratio of (2-15):1 mL / g, heating at a temperature of 100-250° C. for 0.5-5 h, and continuously introducing an oxidizing gas until the oxygen partial pressure is 0.2-6 MPa, obtaining a mixed slurry after the reaction, and then performing solid-liquid separation to obtain a chromium-containing alkali solution and tailings; The oxidizing gas includes air and / or oxygen.

Citation Information

Patent Citations

  • Chromium-containing material strong oxidizing roast technique

    CN101456589A

  • Method for preparing chromate by alkaline roasting carbon ferrochrome

    CN102040245A

  • Method for producing sodium chromate and co-producing chrome-containing cast iron by three-stage process through un-calcium roasting

    CN102557137A

  • Acid leaching pretreatment method for extracting chromium from chromium residues

    CN111139359A

  • Method for extracting chromium from chromite through calcium-free roasting

    CN112875752A