Ultrahigh-strength steel with yield strength of 1300MPa and production method thereof
By adding alloy elements to the steel and adopting two quenching processes, combined with MULPIC rapid cooling device, the strength and toughness of ultra-high strength steel are solved, and the yield strength and toughness of 1300MPa grade ultra-high strength steel is achieved efficiently and at low cost. Improves low-temperature impact toughness and comprehensive performance.
Patent Information
- Application Number
- CN202411473395.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-11-26
AI Technical Summary
When producing ultra-high strength steel with yield strength of 1300MPa grade, it is difficult to take into account the strength and toughness of the steel plate. In addition, the traditional quenching process has problems with the hardenability and welding properties of the steel plate, and the cost is high.
Add alloy elements such as Cr, Ni, Mo and a small amount of Ti and B microalloy elements to the steel. Two quenching processes (online quench + offline quenching) are used to control the cooling rate and temperature through the MULPIC rapid cooling device to form fine martensite Organization, improve low-temperature impact toughness and comprehensive performance.
It has achieved efficient and low-cost production of ultra-high strength steel with yield strength of 1300MPa grade, improved the low-temperature impact toughness and comprehensive performance of steel plates, simplified the process flow, reduced production costs, and the steel plate has good thermal stability and market competitiveness.
Smart Images

Figure CN119020697A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of steel materials, in particular to ultra-high strength steel with a yield strength of 1300 MPa and a production method thereof. Background Art
[0002] Ultra-high-strength steel with a yield strength of 1300MPa not only requires the steel plate to have extremely high strength, but also requires it to have good plasticity, welding formability and plate flatness. It is extremely difficult to produce. This type of steel plate is mainly used in the manufacturing of ultra-large engineering machinery, mining machinery, cement chemical industry and other equipment.
[0003] The post-rolling DQ direct quenching process is often used in the production of quenched and tempered steel with a tensile strength of more than 700MPa. Compared with the traditional offline quenching and tempering process, the online quenching process uses a faster cooling rate and a lower terminal cooling temperature after rolling, so that the steel plate does not undergo ferrite and pearlite phase transformation, and directly enters the bainite or martensite transformation zone, forming a microstructure dominated by refined bainite or martensite, which has higher strength and toughness.
[0004] Therefore, whether the quenching process can be used in the production of ultra-high-strength steel to improve the strength of the steel and ensure the various properties of the steel has been a research direction in recent years. Summary of the invention
[0005] The purpose of the present invention is to provide an ultra-high strength steel with a yield strength of 1300MPa and a production method thereof. The present invention strengthens the steel plate by adding alloy elements such as Cr, Ni, Mo and a small amount of Ti and B micro-alloy elements to the steel, and adopts a double quenching process (online quenching + offline quenching). While reducing precious alloy elements such as Ni, the problem of balancing the strength and toughness of the steel plate and the hardenability of the steel plate is solved, the low-temperature impact toughness of the steel plate is effectively improved, good comprehensive performance is obtained, and efficient and low-cost production of ultra-high strength steel with a yield strength of 1300MPa is achieved.
[0006] The invention discloses an ultra-high strength steel with a yield strength of 1300 MPa, comprising the following chemical components in percentage by mass: C: 0.17-0.19%, Si: 0.20-0.30%, Mn: 0.90-1.10%, P≤0.012%, S≤0.003%, As≤0.007%, Als: 0.020-0.035%, Nb: 0.015-0.035%, Cr: 0.35-0.50%, Ni: 0.70-0.90%, Mo: 0.40-0.60%, Ti: 0.010-0.020%, B: 0.0008-0.0020%, N≤0.0045%, and the rest are Fe and unavoidable impurities.
[0007] The ultra-high strength steel finished product plate produced by the present invention has a thickness specification of 16-30 mm, a yield strength of ≥1300 MPa, a tensile strength of ≥1350 MPa, an elongation after fracture A of ≥8%, and an impact energy of ≥50 J at -40°C.
[0008] A method for producing ultra-high strength steel with a yield strength of 1300 MPa of the present invention comprises the following steps: (1) Steelmaking: adopt the "converter-LF furnace-RH furnace-continuous casting" process to cast ingots with appropriate cross-sections; (2) Heating of the ingot: The ingot is heated to 1230-1290°C and the furnace temperature is 1190-1230°C; (3) Two-stage rolling: In the first stage, ordinary rolling is adopted, and continuous rolling is carried out with a large reduction rate in the rough rolling pass. The total number of passes in the rough rolling stage is ≤7, and the total reduction rate is ≥60% to ensure dynamic recrystallization of the deformed metal and refinement of the austenite grains; in the second stage, the starting rolling temperature is 980-1030℃, and the final rolling temperature is 910-950℃; (4) First quenching: After the steel plate is rolled and passes through the pre-straightening machine, it enters the MULPIC area for DQ strong cooling. The cooling temperature is ≥800℃, the roller speed is controlled at 1.0-1.2m / s, the cooling rate is 21-50℃ / S, and the red-return temperature after strong cooling is ≤200℃. The specific operating parameters of the MULPIC rapid cooling device vary according to the steel plate thickness H, as shown in the following table: ; (5) The steel plate is subjected to a second quenching heat treatment, with a quenching temperature of 835±10℃ and a holding time of H+30min, where H is the thickness of the steel plate. The second quenching can reduce the residual austenite, obtain fine martensite, effectively improve the low-temperature impact toughness of the steel plate, and obtain good comprehensive performance.
[0009] When the MULPIC rapid cooling device is used in the above step (4), the head and tail shields are closed and the spray is used normally; when the water temperature is ≥26°C, the cooling tower needs to be opened in advance for cooling.
[0010] The MUPLIC rapid cooling device described in the present invention adopts a variable flow water pillow cooling header with edge shielding and water convexity control, with 24 headers arranged at the top and bottom, divided into 4 zones A, B, C, and D, each zone is 6 meters long, with a total length of 24 meters. It has an online quenching function and adopts a fully automatic cooling model control. According to the performance requirements of each steel grade, by setting the start cooling temperature, the final cooling temperature, and the cooling rate, the water volume of each header, the upper and lower water ratio, the roller speed and other process parameters can be automatically controlled.
[0011] The reasons for limiting the amounts of the main chemical components of the steel of the present invention are as follows: C: Carbon plays a major role in solid solution strengthening in steel and is the most suitable element for strengthening steel. However, if the carbon content is too high, it will not only damage the plastic toughness, resistance to temper embrittlement, hydrogen embrittlement and fatigue performance of the steel plate, but more importantly, it will seriously damage the weldability of the steel plate. The C content of the present invention is controlled at 0.17-0.19%.
[0012] Si: Si is a commonly used deoxidizer. In quenched and tempered steel, it can not only significantly improve the hardenability of the steel plate, but also improve the tempering resistance of the quenched steel. Too high Si content will affect the plasticity and weldability of the steel plate. The Mn content of the present invention is controlled at 0.20-0.30%.
[0013] Mn: solid dissolves in ferrite and austenite, expands the austenite region, reduces the phase transition point during cooling, improves the hardenability of steel, and significantly improves the strength and hardness of steel, but has an unfavorable tendency to increase grain coarsening and temper brittleness. The Mn content of the present invention is controlled at 0.90-1.10%.
[0014] Cr: Cr is an alloy element that improves hardenability in high-strength steel, especially when reasonably matched with elements such as Mn and Si, the hardenability is significantly increased. During online quenching, Cr is dissolved in martensite, which can improve the tempering resistance of the steel plate. However, when the amount of Cr added is too much, the weldability and temper brittleness resistance of the steel plate are seriously damaged. The Cr content of the present invention is controlled at 0.35-0.50%.
[0015] Nb: Nb can significantly increase the austenite recrystallization temperature of steel, expand the range of the non-recrystallization zone, facilitate high-temperature rolling, and benefit the subsequent online quenching process performance and plate shape. Nb can also inhibit the growth of austenite grains, and has significant fine grain strengthening and precipitation strengthening effects, which provides a basis for the steel plate to still have a fine structure after quenching and tempering, which is beneficial to improving toughness. However, due to the limit of C content and heating temperature, too high Nb cannot be dissolved and deteriorates welding performance. The Nb content of the present invention is controlled to be 0.015-0.035%.
[0016] Ni: Improves plasticity and toughness (improves low-temperature toughness more significantly), improves corrosion resistance, and is used in combination with chromium and molybdenum to improve thermal strength. It is one of the main alloying elements of heat-resistant steel and stainless acid-resistant steel. The Ni content of the present invention is controlled to be 0.70-0.90%.
[0017] Mo: Improves the hardenability of steel. When the content is 0.5%, it can reduce temper brittleness and has a secondary hardening effect. Improves thermal strength and creep strength. When the content is 2% to 3%, it improves the corrosion resistance of organic acids and reducing media. The Mo content of the present invention is controlled at 0.40 to 0.60%.
[0018] Ti: Ti element can play the role of dispersion strengthening and grain refinement, can inhibit the growth of grains in the high temperature zone, and hinder the coarsening of austenite during high temperature heating. When the content is high, it is easy to form large particles of TiN precipitates, which seriously deteriorate the low temperature impact toughness. The Ti content of the present invention is controlled to be 0.010-0.020%.
[0019] B: B is an important component in high-strength quenched and tempered steel. It can improve the hardenability of steel. Adding a very small amount of B will have a significant effect, significantly delaying the transformation of austenite to ferrite and pearlite. When Nb is present at the same time, the effect of B is more prominent. When the B content is less than 0.0005%, the effect of improving hardenability is not great; when the B content is 0.008%, the structure of the steel will be more easily transformed into martensite. The B content of the present invention is controlled at 0.0008-0.0020%.
[0020] P and S: Both are harmful inclusion elements in steel grades, which are easy to form defects such as inclusions and segregation, affecting the impact toughness, elongation, weldability and Z-direction performance of the steel plate. Considering practical operability, the present invention controls P≤0.012% and S≤0.003%.
[0021] As: As is a harmful element for high-strength tempered steel, which directly affects the elongation and impact toughness of the steel plate. In addition, As has an adverse effect on the welding of alloy steel, and the impact is small when the content is within 0.010%. The present invention strictly controls As≤0.007%.
[0022] N: Control N≤0.0045% to avoid the formation of B nitride, which will make B's hardenability ineffective.
[0023] The reasons for setting the main production process parameters of the steel of the present invention are as follows: (1) The steel plate adopts two-stage controlled rolling. The intermediate billet thickness is mainly set based on the thickness accuracy control in the finishing stage and the refinement and elongation of austenite grains, so as to provide enough nucleation points for the subsequent DQ strong cooling. The setting of the second-stage rolling temperature is mainly based on the austenite recrystallization temperature under the composition conditions. The rolling temperature is increased as much as possible but the mixed crystal rolling is reduced. The setting of the final rolling temperature, on the one hand, lays the foundation for hitting the DQ cooling temperature, so that the matrix maintains the austenite structure before the steel plate enters the water cooling. On the other hand, the higher second-stage rolling temperature can shorten the steel plate waiting time and improve the rolling efficiency.
[0024] (2) The initial cooling temperature of the steel plate is ≥800℃. This is mainly because when the temperature of the steel plate is too high, the core of the steel plate may be heated up and the austenite grains may recrystallize and coarsen. When the initial cooling temperature is too low, the ferrite phase transformation may occur to form a soft ferrite structure, which is not conducive to the DQ strong cooling to form martensite / bainite structure. During the direct quenching process, the original austenite dislocations are inherited into the martensite structure and hinder its shear growth, promoting the refinement of martensite laths and lath bundles. In addition, the use of an increased cooling rate to increase the undercooling of martensite transformation can increase the driving force of phase transformation and obtain a denser nucleation rate. The final cooling temperature should be designed to be ≤200℃.
[0025] (3) The steel plate is quenched for the second time at 835±10℃. Compared with the first quenching, the second quenching may more accurately control the cooling rate and temperature of the steel, thereby forming a more uniform and denser dislocation network within a specific temperature range. These high-density dislocations provide abundant nucleation sites for the subsequent precipitation of carbides. In the presence of high-density dislocations, carbides are more likely to nucleate and grow at these locations because dislocations reduce the energy required for nucleation, allowing carbides to precipitate preferentially at these locations. The precipitated fine carbides can significantly enhance the strength of the steel plate. As hard points, these carbides can hinder the movement of dislocations, thereby increasing the yield strength and tensile strength of the material. At the same time, because the carbide particles are small and evenly distributed, they have little effect on the toughness and plasticity of the material. The precipitated fine carbides usually have high thermal stability and can maintain their morphology and distribution at high temperatures. This stability enables the steel plate to maintain good mechanical properties at high temperatures.
[0026] In summary, when the steel plate is quenched for the second time at 835±10℃, high-density dislocations are formed to provide nucleation points for carbide precipitation, which promotes the precipitation of fine and stable carbides. These carbides not only enhance the strength of the steel plate, but also improve its high-temperature tempering resistance by pinning dislocations. This microstructural change enables the steel plate to maintain excellent mechanical properties at high temperatures.
[0027] The beneficial effects of the present invention are as follows: (1) The ultra-high strength steel with a yield strength of 1300 MPa produced by the present invention has excellent comprehensive performance, does not require tempering heat treatment, effectively shortens the process flow and production costs, and is easy to carry out large-scale production.
[0028] (2) The present invention makes full use of various strengthening mechanisms such as alloy solid solution strengthening, grain refinement strengthening, phase transformation strengthening, dislocation strengthening, etc., and realizes a double quenching process (online quenching + offline quenching) through a MULPIC rapid cooling device. The stability of austenite in the first quenching is relatively strong, so there is more residual austenite after quenching; during the second quenching, it is only necessary to heat to a suitable temperature and keep the heat preservation time short, so that the grains can be refined and cryptocrystalline martensite can be presented, thereby obtaining the best comprehensive performance, maximizing the potential of various components in steel and various equipment in production, and making the steel plate have higher thermal stability, lower production cost, stronger market competitiveness, and broad prospects, making outstanding contributions to improving the economic benefits of enterprises. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a metallographic structure diagram (100 μm) of a 16 mm steel plate prepared in Example 1 of the present invention after secondary quenching; Figure 2 This is a metallographic structure diagram (20 μm) of a 16 mm steel plate prepared in Example 1 of the present invention after secondary quenching. DETAILED DESCRIPTION
[0030] In order to better explain the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with specific embodiments. The following embodiments are merely exemplary of the technical solution of the present invention and do not limit the present invention in any form. The serial numbers of the following embodiments are only for description and do not represent the advantages and disadvantages of the embodiments.
[0031] Table 1 below is a list of chemical composition values of steel plates of various embodiments of the present invention (wt, %); Table 2 below is a list of main process parameter values for the steel plate heating and rolling processes of various embodiments of the present invention; Table 3 below is a list of main process parameter values of the steel plate heat treatment process of various embodiments of the present invention; Table 4 below is a list of the second quenching parameters of the steel plates of various embodiments of the present invention and the main mechanical properties test results of the finished steel plates.
[0032] A method for producing ultra-high strength steel with a yield strength of 1300 MPa in each embodiment of the present invention comprises the following steps: (1) Steelmaking: adopt the "converter-LF furnace-RH furnace-continuous casting" process to cast ingots with appropriate cross-sections; (2) Heating of the ingot: The ingot is heated to 1230-1290°C and the furnace temperature is 1190-1230°C; (3) Two-stage rolling: In the first stage, ordinary rolling is adopted, and continuous rolling is carried out with a large reduction rate in the rough rolling pass. The total number of passes in the rough rolling stage is ≤7, and the total reduction rate is ≥60% to ensure dynamic recrystallization of the deformed metal and refinement of the austenite grains; in the second stage, the starting rolling temperature is 980-1030℃, and the final rolling temperature is 910-950℃; (4) First quenching: After the steel plate is rolled and passes through the pre-straightening machine, it enters the MULPIC area for DQ strong cooling. The cooling temperature is ≥800℃, the roller speed is controlled at 1.0~1.2m / s, the cooling rate is 21~50℃ / S, and the red-return temperature after strong cooling is ≤200℃. The specific operating parameters of the MULPIC rapid cooling device vary according to the steel plate thickness value H, as shown in the following table: ; (5) The steel plate is subjected to a second quenching heat treatment, with a quenching temperature of 835±10℃ and a holding time of H+30min, where H is the thickness of the steel plate. The second quenching can reduce the residual austenite, obtain fine martensite, effectively improve the low-temperature impact toughness of the steel plate, and obtain good comprehensive performance.
[0033] When the MULPIC rapid cooling device is used in the above step (4), the head and tail shields are closed and the spray is used normally; when the water temperature is ≥26°C, the cooling tower needs to be opened in advance for cooling.
[0034] The MUPLIC rapid cooling device described in each embodiment of the present invention adopts a variable flow water pillow cooling header with edge shielding and water convexity control, 24 of which are arranged at the top and bottom, divided into 4 zones A, B, C, and D, each zone is 6m, with a total length of 24m, and has an online quenching function. It adopts a fully automatic cooling model control. According to the performance requirements of each steel grade, by setting the start cooling temperature, the final cooling temperature, and the cooling rate, the water volume of each header, the upper and lower water ratio, the roller speed and other process parameters can be automatically controlled.
[0035] Table 1 List of chemical composition values of steel plates of various embodiments of the present invention (wt, %)
[0036] Table 2 List of main process parameter values of steel plate heating and rolling process in various embodiments of the present invention
[0037] Table 3 List of main process parameter values of the steel plate heat treatment process of each embodiment of the present invention
[0038] Table 4 List of the second quenching parameters of the steel plates of various embodiments of the present invention and the main mechanical properties test results of the finished steel plates
[0039] As can be seen from Tables 1 to 4, the steel plates with a thickness of 16 to 30 mm produced in Examples 1 to 5 of the present invention are strengthened by adding alloy elements such as Cr, Ni, Mo and a small amount of Ti and B microalloy elements to the steel, and the two-time quenching process (online quenching + offline quenching) is adopted to effectively improve the low-temperature impact toughness of the steel plate, obtain good comprehensive performance, and have uniform and stable performance, meet the performance requirements of "yield strength ≥ 1300MPa, tensile strength ≥ 1350MPa steel plate, elongation after fracture A ≥ 8%, -40℃ impact energy ≥ 50J", and realize efficient and low-cost production of ultra-high strength steel with a yield strength of 1300MPa. This steel is difficult to produce, has strong market competitiveness, and has broad prospects.
[0040] Figure 1 and Figure 2 They are respectively the metallographic organization diagrams (100 μm) and (20 μm) of the 16 mm specification steel plate prepared in Example 1 of the present invention after secondary quenching. It can be seen from the figures that the structure of the steel plate is martensite with good uniformity.
[0041] The above embodiments are only specific examples for explaining the present invention and do not limit the present invention in any form. Any non-substantial changes made by anyone based on the above contents and forms without departing from the protection scope of the claims of the present invention shall be deemed to fall within the protection scope of the claims of the present invention. The present invention is not limited to the above specific implementation examples.
Claims
1. An ultra-high strength steel with a yield strength of 1300 MPa, characterized in that The invention relates to a nickel-based alloy comprising the following chemical compositions in percentage by mass: C: 0.17-0.19%, Si: 0.20-0.30%, Mn: 0.90-1.10%, P≤0.012%, S≤0.003%, As≤0.007%, Als: 0.020-0.035%, Nb: 0.015-0.035%, Cr: 0.35-0.50%, Ni: 0.70-0.90%, Mo: 0.40-0.60%, Ti: 0.010-0.020%, B: 0.0008-0.0020%, N≤0.0045%, and the rest are Fe and unavoidable impurities.
2. The ultra-high strength steel with a yield strength of 1300 MPa according to claim 1, characterized in that: The ultra-high strength steel finished plate has a thickness specification of 16 to 30 mm, a yield strength ≥1300 MPa, a tensile strength ≥1350 MPa, an elongation after fracture A ≥8%, and an impact energy at -40°C ≥50 J.
3. A method for producing ultra-high strength steel with a yield strength of 1300 MPa as claimed in claim 1 or 2, characterized in that The steps include: (1) Steelmaking: adopt the "converter-LF furnace-RH furnace-continuous casting" process to cast ingots with appropriate cross-sections; (2) Heating of the ingot: The ingot is heated to 1230-1290°C and the furnace temperature is 1190-1230°C; (3) Two-stage rolling: In the first stage, ordinary rolling is adopted, and continuous rolling is carried out with a large reduction rate in the rough rolling pass. The total number of passes in the rough rolling stage is ≤7, and the total reduction rate is ≥60% to ensure dynamic recrystallization of the deformed metal and refine the austenite grains. The starting rolling temperature in stage II is 980-1030°C, and the final rolling temperature is 910-950°C; (4) First quenching: After the steel plate is rolled and passes through the pre-straightening machine, it enters the MULPIC area for DQ strong cooling. The cooling temperature is ≥800℃, the roller speed is controlled at 1.0-1.2m / s, the cooling rate is 21-50℃ / S, and the red-return temperature after strong cooling is ≤200℃. The specific operating parameters of the MULPIC rapid cooling device vary according to the steel plate thickness H, as shown in the following table: ; (5) The steel plate is subjected to a second quenching heat treatment, with a quenching temperature of 835±10℃ and a holding time of H+30min, where H is the thickness of the steel plate.
4. The method for producing ultra-high strength steel with a yield strength of 1300 MPa according to claim 3, characterized in that: When the MULPIC rapid cooling device is used in step (4), the head and tail shields are closed and the spray is used normally; when the water temperature is ≥26°C, the cooling tower is opened in advance for cooling.
5. The method for producing ultra-high strength steel with a yield strength of 1300 MPa according to claim 3, characterized in that: The MUPLIC rapid cooling device adopts a variable flow water pillow cooling header with edge shielding and water convexity control, with 24 headers arranged at the top and bottom, divided into 4 zones A, B, C, and D. Each zone is 6 meters long and has a total length of 24 meters. It has an online quenching function and adopts a fully automatic cooling model control. According to the performance requirements of each steel grade, the water volume of each header, the upper and lower water ratio, and the roller speed can be automatically controlled by setting the start cooling temperature, the final cooling temperature, and the cooling rate.