Novel low-yield-ratio Q420qE steel plate and manufacturing method thereof

By reasonably controlling the chemical composition and process flow in Q420qE steel plate, the problems of unstable steel plate performance and poor plate shape in traditional production are solved, the stability of tensile strength and yield strength and the improvement of plate shape are achieved, and the production cost is reduced and improve efficiency.

CN119020702APending Publication Date: 2024-11-26BAOSTEEL ZHANJIANG IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411145391.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

There are problems of unstable performance and poor plate shape in the traditional Q420qE steel plate production process, which leads to large fluctuations in the tensile strength and yield strength ratios, affecting production efficiency.

Method used

Adopt specific chemical composition combinations and manufacturing process flows, including reasonable content control of C, Si, Mn, Nb, Ti, Cr, as well as blast furnace water molten iron, converter smelting, LF+RH refining, slab continuous casting, rolling mill rolling and rapid Cooling process, controlling the outlet temperature, furnace time, rolling mill rolling temperature and cooling rate, and using DQ cooling process to ensure uniformity and plate shape of the steel plate.

Benefits of technology

The stable performance and good plate shape of the steel plate are achieved, and the tensile strength and yield strength are controlled within a small range, which reduces the temperature difference and unevenness of the plate surface, avoids the heat treatment tempering process, and improves production efficiency and cost-effectiveness. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a novel Q420qE steel plate with a low yield ratio. The novel Q420qE steel plate is prepared from chemical components in percentage by mass as follows: 0.04%-0.06% of C, 0.2%-0.3% of Si, 1.48%-1.56% of Mn, 0.030%-0.045% of Nb, 0.011%-0.017% of Ti, 0.05%-0.13% of Cr, 0%-0.015% of P, 0%-0.002% of S and the balance of Fe and inevitable impurities. The invention further provides a manufacturing method of the steel plate. The manufacturing method comprises the following technological processes of blast furnace molten iron preparation, molten iron pretreatment, converter smelting, LF + RH refining, slab continuous casting, casting blank cleaning, slab heating, rolling mill rolling, rapid cooling and slow cooling. The alloy is low in use cost and has the advantage of being capable of being produced on a large scale; according to the method, the strength of the steel plate can be well controlled, the results of qualified yield ratio, stable performance and good plate shape are achieved in a low final cooling mode, the temperature uniformity of the steel plate is improved, the strength of the steel plate is adjusted without a heat treatment tempering procedure, and a low-cost and high-efficiency production mode is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgical process, and in particular to a novel low-yield ratio Q420qE steel plate and a manufacturing method thereof. Background Art

[0002] At present, the performance requirements and production status of low yield ratio Q420qE steel plates are aimed at, especially the upper and lower limits of tensile strength are set, the range of performance fluctuation is controlled within 120MPa, and the yield ratio is higher than that of ordinary Q420qE steel plates, which needs to be controlled within 0.85. The yield ratio of ordinary Q420qE steel plates is required to be within 0.88. According to the traditional production process, the final cooling temperature between 400 and 550℃ is adopted, and the performance fluctuation of the steel plate is large. There are 8% of the samples with yield ratio exceeding the upper limit. At the same time, the plate shape of the steel plate is poor. After rolling, the reverse wave appears on the cooling bed, which affects the smooth flow of finishing logistics and reduces the overall production efficiency. The Q420qE steel plates produced by the traditional process today have the problem of unstable performance, and generally need to be rescued by additional heating treatment process, which is not conducive to large-scale production. There are also problems with poor plate shape, which is not conducive to the rapid logistics of steel plates, making the production line production efficiency low. Summary of the invention

[0003] The purpose of the present invention is to provide a novel low yield ratio Q420qE steel plate and a manufacturing method thereof, which can solve the problems of unstable performance and poor plate shape existing in the Q420qE steel plate produced by traditional technology.

[0004] In order to achieve the above object, the present invention adopts the following technical solution: A novel low yield ratio Q420qE steel plate, the chemical composition of which, by mass percentage, includes: C: 0.04-0.06%, Si: 0.2-0.3%, Mn: 1.48-1.56%, Nb: 0.030-0.045%, Ti: 0.011-0.017%, Cr: 0.05-0.13%, P: 0-0.015%, S: 0-0.002%, and the remaining components are Fe and unavoidable impurities.

[0005] The main functions and design basis of the chemical elements of the new low yield ratio Q420qE steel plate described in the present invention are: C: C is the most basic strengthening element. C dissolves in steel to form interstitial solid solution, which plays a role in solid solution strengthening. It forms carbide precipitation with strong carbide forming elements or forms carbides, which plays a role in precipitation strengthening. However, too high C content is not good for the toughness and welding performance of steel; too low C content will reduce the strength of steel. Therefore, the C content control range of the present invention is 0.04-0.06%.

[0006] Si: Si is a solid solution strengthening element and also a deoxidizing element in steel, but too high Si content will deteriorate the welding performance of steel and is not conducive to the removal of hot rolling scale during rolling. Therefore, the Si content of the present invention is controlled within a range of 0.2 to 0.3%.

[0007] Mn: Mn improves the strength of steel by solid solution strengthening. It is the most important and economical strengthening element in steel to compensate for the strength loss caused by the reduction of C content. Mn is also an element that expands the γ phase region, which can reduce the γ→α phase transition temperature of steel, help to obtain fine phase transition products, and improve the toughness of steel. However, Mn is an element that is easy to segregate. When the Mn content is high, Mn is easy to segregate in the center of the plate thickness during the casting process. After rolling, a hard phase martensite structure is generated, which reduces the low-temperature toughness and dynamic tear resistance of the material. Therefore, the Mn content control range of the present invention is 1.48-1.56%.

[0008] Nb: Nb is one of the important elements of low-carbon microalloy steel. During the hot rolling process, the Nb dissolved in the solid solution is strain-induced to precipitate to form Nb (N, C) particles, which pin the grain boundaries to inhibit the growth of deformed austenite and inhibit the occurrence of recrystallization. After controlled rolling and controlled cooling, the deformed austenite is transformed into a fine product with a high dislocation density; too low Nb content, the dispersion precipitation effect is not obvious, and it cannot play the role of refining grains and strengthening the matrix; too high Nb content, because it inhibits the occurrence of recrystallization in the core of the steel plate, is not conducive to grain refinement; and the solid solution of Nb is related to the C content. If the C content is too high, the amount of Nb dissolved in the solid solution is small, and the precipitation strengthening and grain sliding effects cannot be achieved; too low C content will lead to grain boundary weakening, and too low Nb content will not have a significant precipitation strengthening effect. Therefore, the control range of the Nb content of the present invention is 0.030-0.045%.

[0009] Ti: Ti is a strong carbonitride-forming element. The undissolved carbonitride of Ti can prevent the growth of austenite grains when the steel is heated. The TiN precipitated during rough rolling in the high-temperature austenite zone can effectively inhibit the growth of austenite grains. In addition, during the welding process, the TiN particles in the steel can significantly prevent the growth of grains in the heat-affected zone, thereby improving the welding performance of the steel plate, and at the same time have a significant effect on improving the impact toughness of the welding heat-affected zone. Therefore, the Ti content control range of the present invention is 0.011-0.017%.

[0010] Cr: Cr is an important element to improve the hardenability of steel, ensure the uniformity of the structure and performance of the steel plate throughout its thickness, and effectively improve the corrosion resistance of steel; however, when too high a content of Cr and Mn is added to steel at the same time, low melting point Cr-Mn composite oxides will be formed, which will form surface cracks during hot working and seriously deteriorate welding performance. Therefore, the Cr content of the present invention is controlled within a range of 0.05 to 0.13%.

[0011] S, P: S and P are inevitable impurity elements in steel, and the lower the better; through ultra-low sulfur (KR stirring desulfurization process, making it less than 20ppm) and Ca treatment, the inclusion morphology of sulfides is controlled, and the P content is controlled below 0.015%, which can ensure that the invented steel has good low-temperature impact toughness.

[0012] Furthermore, the thickness of the novel low yield strength ratio Q420qE steel plate is 10 to 30 mm.

[0013] Furthermore, the mechanical properties of the new low yield ratio Q420qE steel plate are as follows: transverse tensile strength and longitudinal tensile strength are controlled at 570-690 MPa, transverse yield strength and longitudinal yield strength are greater than or equal to 420 MPa, full-size Charpy impact energy at -40°C is greater than or equal to 200 J, cross-sectional shear rate is greater than or equal to 85%, and yield ratio is less than or equal to 0.85.

[0014] The present invention also provides a novel method for manufacturing a low yield ratio Q420qE steel plate, which includes the following process flow: blast furnace molten iron → molten iron pretreatment → converter smelting → LF+RH refining → slab continuous casting → ingot cleaning → slab heating → rolling on a rolling mill → rapid cooling → slow cooling.

[0015] The following process parameters are controlled in the process flow: (1) The furnace temperature is controlled at 1120-1180°C. The design basis is: if the furnace temperature of the steel plate is higher than 1180°C, the temperature will be too high, the state of the iron oxide scale on the surface of the steel plate will deteriorate, and after descaling, the temperature of the steel plate surface will be uneven, resulting in poor uniformity. If the furnace temperature of the steel plate is lower than 1120°C, the rolling difficulty of the steel plate will increase, resulting in poor rolled plate shape, which will affect the cooling and plate shape of the steel plate; (2) The furnace time is greater than 200 minutes. Its main function is to ensure that the alloy of the steel plate is fully dissolved in the slab, reduce the temperature difference of the steel plate as a whole, and make the steel plate fully burned through; (3) The rolling process of the rolling mill includes a rough rolling process and a finish rolling process. The rough rolling process includes three stages: forming, widening and rolling. The total number of rough rolling passes is 8 to 10, wherein the forming and rolling passes are performed with a large reduction. After the rough rolling is completed, an intermediate billet is formed. The intermediate billet is kept warm on the intermediate roller with a waiting thickness of (3 to 5) * t. When the temperature drops to a specified temperature, finish rolling is performed, wherein t is the thickness of the finished steel plate in mm; (4) The finishing rolling start temperature is the temperature at which the steel plate starts rolling in the pre-recrystallization stage. The finishing rolling start temperature is set according to the different thicknesses of the steel plate. The specific calculation formula is: T=-6*H+1059, where T is the finishing rolling start temperature in °C and H is the thickness of the steel plate in mm. (5) The finishing temperature is the temperature of the last rolling pass of the steel plate. The finishing temperature is controlled at 810-860°C to ensure that the temperature at the tail of the steel plate when cooling starts is greater than 720°C. (6) The rapid cooling method is water cooling, specifically using the DQ cooling process or the DQ+ACC two-stage cooling process, where the water flow density of the DQ section is greater than 18L / s / m 2 , water pressure is greater than or equal to 4 bar; (7) The cooling temperature is controlled at 720-810°C to ensure that the steel plate starts cooling in water before phase change occurs; (8) The final cooling temperature is controlled at 100-380°C. The steel plate will form a low-temperature state with uniform temperature in this temperature range, which is conducive to a uniform phase transformation structure state. After cooling, the steel plate has a good shape; (9) The cooling rate is controlled at 45-70℃ / s, which can form a high cooling rate design during the cooling process. During the cooling process, water-steel direct contact cooling is avoided to form a water-air film-steel cooling process, ensuring the formation of a plate surface with uniform temperature; (10) The water volume ratio between the upper and lower surfaces of the steel plate is set to Ftop / Fbot, and the Ftop / Fbot is controlled at 0.85 to 1.10. The edge temperature of the water cooling device is controlled to be 20 to 50°C higher than the temperature of the steel plate body, wherein Ftop is the water flow density on the upper surface of the steel plate, and Fbot is the water flow density on the lower surface of the steel plate.

[0016] Furthermore, in the rapid cooling of the process flow, the water cooling device is evenly divided into 4 sections in the length direction, which are sections A, B, C, and D from the entrance to the exit. Edge shielding devices are installed on both sides of each section, and an edge shield is formed on one side of each section. There are a total of 8 edge shields, and each edge shield can independently control the edge shielding amount. In the process of controlling edge waves and middle waves, a process of staggered edge shielding is constructed. The edge shielding amount decreases from section A, section B, section C, and section D in sequence, and finally the edge temperature of the water cooling device is controlled to be 20 to 50°C higher than the temperature of the steel plate body.

[0017] Furthermore, when the temperature difference of the plate surface of the new low yield ratio Q420qE steel plate is controlled to be less than or equal to 60° C., the unevenness of the new low yield ratio Q420qE steel plate is less than or equal to 15 mm / 2 m.

[0018] Beneficial effects of the present invention: 1. Compared with the prior art, the stability of the steel plate produced by this method is improved. During mass production, the performance fluctuation range of tensile strength and yield strength is controlled within 50MPa, which is better than the performance fluctuation range of 120MPa in the traditional production process.

[0019] 2. The temperature difference of the steel plate surface is controlled within 60°C, and the unevenness of the steel plate can be controlled within 15mm / 2m, effectively improving the temperature uniformity of the steel plate.

[0020] 3. The new low yield ratio Q420qE steel plate is required to be controlled within the thickness range of 10 to 30 mm, which is a relatively thin steel plate. The treatment by this method can avoid the phenomenon of poor steel plate shape due to uneven cooling of the thin steel plate, and reduce the overall difficulty of rolling the thin steel plate.

[0021] 4. The present invention adopts a low alloy chemical composition system, the alloy use cost is low, and it has the advantage of being able to be produced on a large scale; the present invention can well control the strength of the steel plate, and utilizes a low final cooling method to achieve a qualified yield strength ratio, stable performance, and good plate shape. There is no need to adjust the strength of the steel plate through a heat treatment and tempering process, thereby achieving a low-cost, high-efficiency production method. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described below.

[0023] Example 1 and Example 2: The chemical compositions involved in the two embodiments are the same, including, by mass percentage: C: 0.0532%, Si: 0.2362%, Mn: 1.504%, Nb: 0.0318%, Ti: 0.0137%, Cr: 0.066%, P: 0.0096%, S: 0.0009%, and the remaining components are Fe and unavoidable impurities.

[0024] The process flow of the manufacturing method involved in the two embodiments is: blast furnace molten iron→molten iron pretreatment→converter smelting→LF+RH refining→slab continuous casting→casting cleaning→slab heating→rolling on a rolling mill→rapid cooling→slow cooling.

[0025] The rolling dimensions of the steel plate in Example 1 are: thickness × width × length = 14.27mm × 2987mm × 42921mm; based on the process flow involved in the above Example 1, the specific process parameter control setting values ​​include as follows: the furnace temperature is 1145°C; the furnace time is 208min; the intermediate billet thickness is 56mm; the finishing rolling start temperature is 970°C; the finishing rolling end temperature is 840°C; the cooling mode is DQ; the start cooling temperature is 781°C; the final cooling temperature is 250°C; the cooling rate is 65°C / s; plate shape control performance: Ftop / Fbot is controlled at 0.93, Ftop is the water flow density on the upper surface of the steel plate, and Fbot is the water flow density on the lower surface of the steel plate; the edge shielding amount of section A is 80mm, and the edge shielding amount of section B is 32mm.

[0026] The implementation results of Example 1 are: 1. The transverse tensile strength is 668MPa, the longitudinal tensile strength is 667MPa, the transverse yield strength is 527MPa, the longitudinal yield strength is 521MPa, the transverse yield strength ratio is required to be less than or equal to 0.789, the longitudinal yield strength ratio is required to be less than or equal to 0.781, the full-size Charpy impact energy at -40℃ is 243J, and the section shear is 100%.

[0027] 2. The temperature difference of the steel plate surface is controlled at 54°C, and the unevenness of the steel plate is controlled at 13mm / 2m.

[0028] 3. The overall performance of the steel plate is good, and there is no need to go through a heat treatment and tempering process to adjust the strength of the steel plate.

[0029] The rolling dimensions of the steel plate in Example 2 are: thickness × width × length = 16.32mm × 3759mm × 30494mm; based on the process flow involved in the above Example 2, the specific process parameter control setting values ​​include as follows: the furnace temperature is 1141°C; the furnace time is 212min; the intermediate billet thickness is 56mm; the finishing rolling start temperature is 950°C; the finishing rolling end temperature is 840°C; the cooling mode is DQ; the start cooling temperature is 783°C; the final cooling temperature is 250°C; the cooling rate is 65°C / s; plate shape control performance: Ftop / Fbot is controlled at 1.04, Ftop is the water flow density on the upper surface of the steel plate, Fbot is the water flow density on the lower surface of the steel plate, the edge shielding amount of section A is 89mm, and the edge shielding amount of section B is 18mm.

[0030] The implementation results of Example 2 are: 1. The transverse tensile strength is 668MPa, the longitudinal tensile strength is 652MPa, the transverse yield strength is 530MPa, the longitudinal yield strength is 492MPa, the transverse yield strength ratio is required to be less than or equal to 0.793, the longitudinal yield strength ratio is required to be less than or equal to 0.755, the full-size Charpy impact energy at -40℃ is 298J, and the section shear is 100%.

[0031] 2. The temperature difference of the steel plate surface is controlled at 52°C, and the unevenness of the steel plate is controlled at 12mm / 2m.

[0032] 3. The overall performance of the steel plate is good, and there is no need to go through a heat treatment and tempering process to adjust the strength of the steel plate.

Claims

1. A new type of low yield ratio Q420qE steel plate, characterized by: The chemical composition of the novel low yield ratio Q420qE steel plate includes, by mass percentage, C: 0.04-0.06%, Si: 0.2-0.3%, Mn: 1.48-1.56%, Nb: 0.030-0.045%, Ti: 0.011-0.017%, Cr: 0.05-0.13%, P: 0-0.015%, S: 0-0.002%, and the remaining components are Fe and unavoidable impurities.

2. The new low yield ratio Q420qE steel plate according to claim 1 is characterized in that: The thickness of the novel low yield strength ratio Q420qE steel plate is 10 to 30 mm.

3. The new low yield ratio Q420qE steel plate according to claim 1 or 2, characterized in that: The mechanical properties of the new low yield ratio Q420qE steel plate are as follows: transverse tensile strength and longitudinal tensile strength are controlled at 570-690 MPa, transverse yield strength and longitudinal yield strength are greater than or equal to 420 MPa, full-size Charpy impact energy at -40°C is greater than or equal to 200 J, cross-sectional shear rate is greater than or equal to 85%, and yield ratio is less than or equal to 0.

85.

4. A method for manufacturing a new low yield ratio Q420qE steel plate according to any one of claims 1 to 3, characterized in that: The process flow of the manufacturing method includes: blast furnace molten iron→molten iron pretreatment→converter smelting→LF+RH refining→slab continuous casting→casting cleaning→slab heating→rolling on a rolling mill→rapid cooling→slow cooling; The following process parameters are controlled in the process flow: (1) The furnace temperature is controlled at 1120~1180℃; (2) The time in the furnace is greater than 200 minutes; (3) The rolling process of the rolling mill includes a rough rolling process and a finish rolling process. The rough rolling process includes three stages: forming, widening and rolling. The total number of rough rolling passes is 8 to 10, wherein the forming and rolling passes are performed with a large reduction. After the rough rolling is completed, an intermediate billet is formed. The intermediate billet is kept warm on the intermediate roller with a waiting thickness of (3 to 5) * t. When the temperature drops to a specified temperature, finish rolling is performed, wherein t is the thickness of the finished steel plate in mm; (4) Set the finishing rolling start temperature according to the different thickness of the steel plate. The specific calculation formula is: T=-6*H+1059, where T is the finishing rolling start temperature in °C and H is the steel plate thickness in mm; (5) The finishing temperature of finishing rolling is controlled at 810-860°C; (6) Rapid cooling adopts DQ cooling process or DQ+ACC two-stage cooling process, where the water flow density of the DQ section is greater than 18L / s / m 2 , water pressure is greater than or equal to 4 bar; (7) The cooling temperature is controlled at 720-810℃; (8) The final cooling temperature is controlled at 100-380°C; (9) The cooling rate is controlled at 45-70°C / s; (10) The water volume ratio between the upper and lower surfaces of the steel plate is set to Ftop / Fbot, and the Ftop / Fbot is controlled at 0.85 to 1.

10. The edge temperature of the water cooling device is controlled to be 20 to 50°C higher than the temperature of the steel plate body, wherein Ftop is the water flow density on the upper surface of the steel plate, and Fbot is the water flow density on the lower surface of the steel plate.

5. The method for manufacturing the novel low yield ratio Q420qE steel plate according to claim 4, characterized in that: In the rapid cooling of the process flow, the water cooling device is evenly divided into 4 sections in the length direction, namely sections A, B, C, and D from the inlet to the outlet, and edge shielding devices are installed on both sides of each section.

6. The method for manufacturing the novel low yield ratio Q420qE steel plate according to claim 4, characterized in that: When the temperature difference of the plate surface of the new low yield ratio Q420qE steel plate is controlled to be less than or equal to 60° C., the unevenness of the new low yield ratio Q420qE steel plate is less than or equal to 15 mm / 2 m.

Citation Information

Cited By

  • Bridge steel plate and manufacturing method thereof

    CN121592953A