Preparation method of high-quality atomic beam emission structure based on graphene coating

By using graphene coating and oxygen plasma treatment on the atomic beam emission structure, the problems of uneven scattering and active atomic reactions are solved, the collimation of the atomic beam and the accuracy of the sensor are improved, and the emission structure is extended. life.

CN119020748AActive Publication Date: 2024-11-26CHINA STATE SHIPBUILDING CORP NO 707 RES INST
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410973288.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-26
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

In high-precision sensor applications, the existing atomic beam emission structures have reduced atomic beam collimation and blocked emission structures due to uneven scattering of the inner wall and active atomic reaction, which affects the service life and measurement accuracy.

Method used

Graphene coating technology is used to prepare the emission structure by step assembly, first uniformly coating the metal surface, and then forming a microporous structure. The active site of the coating is improved by oxygen plasma treatment and reduce the divergence angle of the atomic beam.

Benefits of technology

It improves the collimation and quality of the atomic beam flow, extends the service life of the emission structure, and improves the measurement accuracy of the sensor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020748A_ABST
    Figure CN119020748A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a high-quality atomic beam emission structure based on a graphene coating film, and the method comprises the steps: 1, bending a metal foil to form a wave plate, and cutting the wave plate and the metal foil into long-strip rectangles with the same size; 2, cleaning the surfaces of the metal foil and the metal waved plate which are cut and formed in the step 1; 3, the cleaned metal foil and the cleaned metal waved plate are placed in a reaction area of a low-pressure chemical vapor deposition system, and controllable graphene coating is conducted on the surface of the metal foil and the surface of the metal waved plate; 4, taking out the coated metal foil and the metal waved plate, and carrying out measurement characterization; 5, treating the surface of the graphene coating film by using oxygen plasma; and 6, sequentially stacking the metal foil and the metal waved plate up and down, inserting the stacked metal foil and metal waved plate into a square hole of a cylindrical shell, and forming an emission micropore structure inside to complete the preparation of the atomic beam emission structure. According to the invention, the coating difficulty of graphene in micropores is reduced, and the uniformity of coating is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of atomic physics, and specifically relates to a method for preparing a high-quality atomic beam emission structure based on graphene coating. Background Art

[0002] Atomic beams have broad application prospects in atomic physics, chemical physics, and surface physics. The technology of using an atomic furnace to produce high-atom flux, high-collimation, high-quality atomic beams through an emission structure composed of a microtube array has been applied to precision sensors such as atomic clocks and atomic beam gyroscopes. As one of the main factors restricting the measurement accuracy of sensors, with the improvement of sensor accuracy requirements, people's requirements for beam quality are also getting higher and higher. Large-flux atomic beams are subject to uneven scattering by the inner wall of the emission structure and the reaction of active atoms with the inner wall of the emission structure, which will not only cause a decrease in the collimation of the atomic beam, but also cause the emission structure to be blocked in severe cases, affecting the service life of the emission structure. Therefore, it is urgent to design a method for preparing an emission structure to solve the above problems and achieve the preparation of high-quality atomic beams. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention provides a method for preparing a high-quality atomic beam emission structure based on graphene coating.

[0004] The above-mentioned object of the present invention is achieved by the following technical solutions:

[0005] A method for preparing a high-quality atomic beam emission structure based on graphene coating, wherein the emission structure is manufactured by step-by-step assembly to achieve uniform coating of graphene, and the preparation method comprises the following steps:

[0006] Step 1: bend the metal foil to form a corrugated plate, and cut the corrugated plate and the metal foil into long rectangles of equal size according to experimental requirements;

[0007] Step 2: Clean the surface of the metal foil and the corrugated metal plate cut and formed in step 1 to remove the surface particle impurities caused by the material body and machining;

[0008] Step 3, placing the cleaned metal foil and the metal corrugated plate in a reaction area of ​​a low-pressure chemical vapor deposition system, and performing controllable coating of graphene on the surfaces of the metal foil and the metal corrugated plate;

[0009] Step 4, taking out the coated metal foil and the metal corrugated plate and performing measurement and characterization;

[0010] Step 5: Using oxygen plasma to treat the surface of the graphene coating;

[0011] Step 6: stack the metal foil and the metal corrugated plate in sequence, and insert them into the square hole of a cylindrical shell to form an emission micropore structure inside, thereby completing the preparation of the atomic beam emission structure.

[0012] Furthermore, in step 1, the metal foil is bent to form a corrugated plate which is pressed and formed by a set of relatively rotating sawtooth rollers.

[0013] Furthermore, in step 2, acetone, isopropanol, and deionized water are used for cleaning in sequence, and each medium is cleaned for 15 minutes.

[0014] Furthermore, step 3 specifically includes:

[0015] After placing the cut and cleaned metal foil and metal corrugated plate into the reaction zone of the low-pressure chemical vapor deposition system, first use a mechanical pump to pump the gas pressure in the reaction zone to less than 1Pa; then introduce 20sccm argon and raise the temperature to 1000°C; then replace the introduced gas with a mixed gas of 5ccm methane and 2sccm hydrogen, and react for about 10 minutes; finally, replace the introduced gas with 20sccm argon, and quickly cool the system to room temperature.

[0016] Furthermore, step 4 includes:

[0017] The Raman spectrum of graphene is measured using a confocal Raman microscope to characterize the quality and thickness of the graphene coating, and the uniformity of graphene is characterized by Raman spectrum scanning at multiple locations; the surface roughness of graphene is measured using an atomic force microscope.

[0018] Moreover, in step 5, the metal foil and the metal corrugated plate coated with the graphene film are placed in an oxygen plasma treatment system, and the oxygen pressure is controlled to be 0.1 Pa, the power is 100 W, and the treatment time is 3 minutes.

[0019] The advantages and positive effects of the present invention are:

[0020] This preparation method adopts the method of first coating the metal surface with graphene and then making the microporous emission structure, which reduces the difficulty of coating the graphene in the micropores and improves the uniformity of the coating. The introduction of graphene as a coating material effectively reduces the roughness of the inner surface of the atomic emission structure. At the same time, the highly chemically stable graphene avoids the reaction between the atoms and the metal of the emission structure. The graphene treated with oxygen plasma can increase a large number of active sites, adsorb atoms with large divergence angles, and improve the collimation of the atomic beam, thereby effectively improving the quality of the atomic beam passing through the atomic beam emission structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is a schematic cross-sectional view of an atomic beam emission structure made by the present invention;

[0022] Figure 2 It is a schematic diagram of pressing a metal corrugated plate in the atomic beam emission structure of the present invention;

[0023] Figure 3 is the Raman spectrum data of graphene synthesized on the surface of the stainless steel corrugated plate according to the embodiment of the present invention;

[0024] Figure 4 It is a schematic diagram of the use of the atomic emission structure of the present invention.

[0025] Figure 5 Fluorescence images of the atomic beam formed by the emission structure before (a) and after (b) graphene coating. DETAILED DESCRIPTION

[0026] The structure of the present invention is further described below with reference to the accompanying drawings and by way of examples. It should be noted that the present examples are descriptive rather than restrictive.

[0027] A method for preparing a high-quality atomic beam emission structure based on graphene coating, see Figure 1-Figure 4 The invention point is: by assembling the emission structure in steps, the uniform coating of graphene can be achieved. The preparation method of the present invention comprises the following steps:

[0028] Step 1: Bend the metal foil to form a corrugated plate, and cut the corrugated plate and the metal foil into long rectangular strips according to the experimental requirements. The metal foil can be made of stainless steel, copper, nickel, tungsten and other metals, and the thickness can be 0.05mm-0.2mm.

[0029] In this embodiment, a stainless steel foil with a thickness of 0.05 mm was cut into strips of 2 cm × 10 cm and placed in a Figure 2 The pressed stainless steel corrugated plate is cut along the indentation direction to form 2mm×2cm strips, and stainless steel foils with the same size (referring to the plane projection size) are cut at the same time.

[0030] Step 2: Clean the surface of the metal foil 2 and the metal corrugated plate 1 cut and formed in step 1 to remove the surface particle impurities caused by the material body and machining.

[0031] In this embodiment, acetone, isopropanol, and deionized water are used for cleaning for 15 minutes in sequence. Acetone and isopropanol can effectively remove oil stains on the metal surface, while deionized water cleaning can avoid the influence of surface organic solvent residues on subsequent graphene coating.

[0032] Step 3: placing the cleaned metal foil and the corrugated metal plate in a reaction area of ​​a low-pressure chemical vapor deposition system, and performing controllable coating of graphene on the surfaces of the metal foil and the corrugated metal plate.

[0033] In this embodiment, after the cut and cleaned metal foil and metal corrugated plate are placed in the reaction zone of the low-pressure chemical vapor deposition system, the pressure of the reaction zone is first pumped to less than 1Pa by a mechanical pump. Low-pressure chemical vapor deposition and coating under a low-pressure environment can increase the uniformity and controllability of the coating; then 20sccm argon is introduced and the temperature is raised to 1000°C; then the introduced mixed gas of 5ccm methane and 2sccm hydrogen is replaced, and the reaction is carried out for about 10 minutes; finally, the introduced gas is replaced with 20sccm argon, and the system is quickly cooled to room temperature. Argon acts as a protective gas during temperature rise and fall, hydrogen is a reducing gas in the reaction process to prevent metal oxidation, and methane acts as a carbon raw material in the graphene synthesis process.

[0034] Step 4: Take out the coated metal foil and metal corrugated plate and measure and characterize them

[0035] In this embodiment, the Raman spectrum of graphene is measured using a confocal Raman microscope to characterize the quality and thickness of the graphene coating, and the uniformity of graphene is characterized by Raman spectrum scanning at multiple locations; an atomic force microscope is used to measure the surface roughness of graphene. The Raman spectrum of the graphene coated in this embodiment is shown in the figure. Figure 3 From the 2p peak position in , it can be seen that graphene was successfully synthesized on the metal foil surface through the above steps.

[0036] Step 5: Use oxygen plasma to treat the surface of the graphene coating.

[0037] In this embodiment, a metal foil and a metal corrugated plate coated with a graphene film are placed in an oxygen plasma treatment system (existing system), the oxygen pressure is controlled to be 0.1 Pa, the power is 100 W, and the treatment time is 3 minutes. The power of the oxygen plasma is set to 50-150 W. Increasing the power of the oxygen plasma can increase the active adsorption sites on the graphene surface. However, when the power exceeds 150 W, the integrity of the graphene will be damaged, the coverage of the surface will be reduced, and its contribution to the improvement of the atomic beam quality will be reduced. Therefore, it is necessary to maintain the oxygen plasma within a reasonable range.

[0038] Step 6: stack the metal foil and the metal corrugated plate in sequence, and insert them into the square hole of a cylindrical shell 3, as shown in FIG. Figure 1 As shown, an emission microporous structure 5.1 is formed inside, and the preparation of the atomic beam emission structure 5 is completed.

[0039] When the atomic beam emission structure is used, the emission structure is connected to the rubidium atomic furnace 6, and the heated rubidium atoms are ejected from the emission structure port to achieve the emission of high-quality rubidium atomic beams. Compared with the emission structure without graphene coating, the fluorescence image of the atomic beam emitted by the emission structure after graphene coating is significantly narrower, and the brightness at the center is close, indicating that the atomic beam has better quality, see Figure 5 .

[0040] Although the embodiments and drawings of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments and drawings.

Claims

1. A method for preparing a high-quality atomic beam emission structure based on graphene coating, characterized in that: The emission structure is manufactured by step-by-step assembly to achieve uniform coating of graphene, and the preparation method comprises the following steps: Step 1: bend the metal foil to form a corrugated plate, and cut the corrugated plate and the metal foil into long rectangles of equal size according to experimental requirements; Step 2: Clean the surface of the metal foil and the corrugated metal plate cut and formed in step 1 to remove the surface particle impurities caused by the material body and machining; Step 3, placing the cleaned metal foil and the metal corrugated plate in a reaction area of ​​a low-pressure chemical vapor deposition system, and performing controllable coating of graphene on the surfaces of the metal foil and the metal corrugated plate; Step 4, taking out the coated metal foil and the metal corrugated plate and performing measurement and characterization; Step 5: Using oxygen plasma to treat the surface of the graphene coating; Step 6: stack the metal foil and the metal corrugated plate in sequence, and insert them into the square hole of a cylindrical shell to form an emission micropore structure inside, thereby completing the preparation of the atomic beam emission structure.

2. The method for preparing a high-quality atomic beam emission structure based on graphene coating according to claim 1, characterized in that: In step 1, the metal foil is bent into a corrugated plate and then pressed into shape by a set of relatively rotating sawtooth rollers.

3. The method for preparing a high-quality atomic beam emission structure based on graphene coating according to claim 1, characterized in that: In step 2, acetone, isopropanol, and deionized water are used for cleaning in sequence, and each medium is used for cleaning for 15 minutes.

4. The method for preparing a high-quality atomic beam emission structure based on graphene coating according to claim 1, characterized in that: Step 3 specifically includes: After placing the cut and cleaned metal foil and metal corrugated plate into the reaction zone of the low-pressure chemical vapor deposition system, first use a mechanical pump to pump the gas pressure in the reaction zone to less than 1Pa; then introduce 20sccm argon and raise the temperature to 1000°C; then replace the introduced gas with a mixed gas of 5ccm methane and 2sccm hydrogen, and react for about 10 minutes; finally, replace the introduced gas with 20sccm argon, and quickly cool the system to room temperature.

5. The method for preparing a high-quality atomic beam emission structure based on graphene coating according to claim 1, characterized in that: Step 4 includes: The Raman spectrum of graphene is measured using a confocal Raman microscope to characterize the quality and thickness of the graphene coating, and the uniformity of graphene is characterized by Raman spectrum scanning at multiple locations; the surface roughness of graphene is measured using an atomic force microscope.

6. The method for preparing a high-quality atomic beam emission structure based on graphene coating according to claim 1, characterized in that: In step 5, the metal foil and the metal corrugated plate coated with the graphene film are placed in an oxygen plasma treatment system, the oxygen pressure is controlled to be 0.1 Pa, the power is 100 W, and the treatment time is 3 minutes.

Citation Information

Patent Citations

  • Neutral atom beam generating device

    CN116685042A

  • Collimation device for reducing disturbing particles and manufacturing method thereof

    CN118073001A

  • Graphene based field effect transistor

    US20140299841A1