Alkaline electrolytic bath, nickel net catalyst coating of alkaline electrolytic bath and spraying process and application of nickel net catalyst coating

By adjusting the spraying direction and angle, the powder utilization rate and adhesion of the nickel mesh catalyst coating were improved, solving the problems of low powder utilization rate and poor thickness uniformity in the existing technology, and realizing the preparation of low-cost and high-efficiency nickel mesh catalyst coating.

CN119020770AInactive Publication Date: 2024-11-26CEMT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411488125.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing nickel mesh catalyst coating spraying process for alkaline electrolytic cells suffers from problems such as low powder utilization, high spraying cost, poor thickness uniformity, and insufficient adhesion.

Method used

After two nickel meshes are stacked, during the first powder spraying, the spray gun direction maintains the same angle with the warp and weft of the nickel mesh and forms a set angle with the normal of the nickel mesh plane. During the second powder spraying, the spray gun direction is rotated with the normal of the nickel mesh plane as the axis for spraying, ensuring high powder utilization and good thickness uniformity.

Benefits of technology

It improves powder utilization, reduces spraying costs, enhances the adhesion between the nickel mesh catalyst coating and the nickel mesh, and improves thickness uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020770A_ABST
    Figure CN119020770A_ABST
Patent Text Reader

Abstract

The invention provides an alkaline electrolytic cell and a nickel net catalyst coating and a spraying process and application thereof, the spraying process comprises the following steps: (1) two nickel nets are laminated and then subjected to first powder spraying, the spraying direction of a spray gun in the first powder spraying keeps the same included angle with the warp and the weft of the nickel net on the top layer, the angle between the top layer nickel mesh and the normal direction of the top layer nickel mesh plane is a set angle theta1; and (2) after the positions of the two nickel nets are exchanged, the normal direction of the nickel net plane serves as the axis, the spraying direction of the spraying gun is rotated till the angle between the spraying direction of the spraying gun and the normal direction of the nickel net plane on the top layer is the set angle theta 2, then second powder spraying is conducted, and the nickel net catalyst coating is obtained. According to the spraying process for the nickel net catalyst coating of the alkaline electrolytic cell, the powder utilization rate is high, and therefore the spraying process has the low spraying cost; in addition, the nickel net catalyst coating prepared through the spraying technology is good in thickness uniformity and high in binding force with the nickel net.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coating preparation, and relates to a spraying process of a nickel mesh catalyst coating of an alkaline electrolytic cell, and in particular to an alkaline electrolytic cell and a nickel mesh catalyst coating and a spraying process and application thereof. Background Art

[0002] Alkaline electrolyzer is the core equipment for producing hydrogen by electrolyzing water in an alkaline environment. Nickel in alkaline electrolyzer has good catalytic activity for hydrogen evolution and is relatively cheap, so it is used in large quantities. In order to improve the efficiency of hydrogen production, the requirements for the catalytic activity of nickel mesh are also constantly increasing. Increasing the contact area between nickel and alkali solution is an effective way to improve the catalytic activity of nickel mesh. In order to increase the specific surface area of ​​nickel mesh, the mainstream technology adopts plasma spraying technology to spray a layer of nickel-aluminum alloy on the nickel mesh. Before plasma spraying, the substrate needs to be sandblasted to make the surface as rough as possible to improve the bonding strength between the coating and the substrate. After spraying, the nickel mesh needs to be immersed in concentrated alkali solution to dissolve the aluminum and form porous nickel. This process is called activation.

[0003] The substrate for catalyst spraying is usually a woven nickel mesh. Due to the presence of mesh holes, a large amount of powder passes through the mesh holes during spraying and cannot adhere to the nickel mesh, resulting in low powder utilization. The powder utilization rate of conventional spraying processes is generally below 30%. The powder that is not sprayed onto the nickel mesh cannot be collected for secondary spraying due to factors such as high-temperature oxidation, resulting in high spraying costs. In addition, the powder-receiving surface of the nickel wire is an arc-shaped surface. Compared with a flat surface, there are phenomena such as uneven coating thickness on the surface and inconsistent bonding conditions at various positions, which lead to problems such as insufficient bonding strength of the catalytic layer at weak spraying locations and easy falling off during service.

[0004] CN101866795A discloses a method for preparing a nickel mesh cathode. The method first sprays a carbonate suspension on the surface of the nickel mesh cathode to obtain a dense coating on the surface of the nickel mesh cathode with good coating bonding and adhesion and not easy to fall off. Then, the nickel mesh cathode is subjected to exhaust processing. Finally, the nickel mesh cathode is subjected to aging treatment. The obtained nickel mesh cathode has significantly improved emission capacity, longer service life, can be used on high-energy machines for a long time, and has better economic benefits.

[0005] CN115198270A discloses a high temperature resistant nickel-based melt-sprayed composite mesh and its preparation method and application. The high temperature resistant nickel-based melt-sprayed composite mesh of the invention is prepared by the following method: chromium plating: take a clean nickel mesh, electroplate metal chromium on the surface of the nickel mesh to form a chromium plating layer; spraying: spray composite metal powder on the surface of the chromium plating layer to form a bonding layer, and then spray yttrium-stabilized zirconium oxide to form a ceramic layer, so as to obtain a high temperature resistant nickel-based melt-sprayed composite mesh; the composite metal powder is MCrAlY composite metal powder, M is Ni and / or Co, and the content of Al is 10-20wt%. The composite mesh of the invention has the advantages of high temperature resistance, corrosion resistance, long service life, and resistance to rapid temperature rise and fall. The use of the composite mesh to fire MLCC products can improve the product qualification rate.

[0006] The currently disclosed spraying processes of nickel mesh catalyst coatings for alkaline electrolytic cells all have certain defects, such as low powder utilization, resulting in high spraying costs, and poor thickness uniformity of the prepared nickel mesh catalyst coatings and poor bonding strength with the nickel mesh. Therefore, it is very important to develop and design a new type of nickel mesh catalyst coating for alkaline electrolytic cells and its spraying process. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an alkaline electrolytic cell and a nickel mesh catalyst coating and a spraying process and application thereof. The powder utilization rate of the spraying process of the nickel mesh catalyst coating of the alkaline electrolytic cell provided in the present invention is high, so that the spraying process has a lower spraying cost; in addition, the nickel mesh catalyst coating prepared by the spraying process has good thickness uniformity and strong bonding with the nickel mesh.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, the spraying process comprising:

[0010] (1) After stacking two nickel meshes, a first powder spraying is performed, wherein the spraying direction of the spray gun in the first powder spraying maintains the same angle with the warp and weft of the nickel mesh of the top layer, and the angle with the normal direction of the plane of the nickel mesh of the top layer is a set angle θ1;

[0011] (2) After the positions of the two nickel meshes are swapped, the spray direction of the spray gun is rotated to a set angle θ2 with the normal direction of the nickel mesh plane as the axis, and then a second powder spraying is performed to obtain a nickel mesh catalyst coating.

[0012] In the present invention, the spraying direction of the spray gun in the first powder spraying maintains the same angle with the warp and weft of the nickel mesh on the top layer, and the angle with the normal direction of the plane of the nickel mesh on the top layer is a set angle θ1, so the projection area of ​​the hole area perpendicular to the spraying direction is also smaller than the area of ​​the mesh, reducing the amount of powder leaking through the mesh and improving the powder utilization rate.

[0013] During the first powder spraying in the present invention, the top nickel mesh is mainly sprayed, but part of the powder leaking from the mesh holes of the top nickel mesh will be received by the top nickel mesh, thereby reducing the waste of powder and improving the powder application rate; after the first powder spraying is completed, the two nickel meshes are exchanged, the original bottom nickel mesh is placed on top, and then the spray direction of the spray gun is rotated to θ2 as the new spray direction with the normal direction of the plane of the top nickel mesh as the axis, and the second powder spraying is performed to reach the preset powder application amount.

[0014] In the present invention, the directions of the first powder spraying and the second powder spraying do not completely overlap, the thickness at the thickest part of the top is reduced, the internal stress is reduced, the overall thickness distribution is relatively more uniform, the proportion of the area with moderate thickness is increased, and the bonding force between the coating and the nickel mesh is enhanced.

[0015] The powder utilization rate of the spraying process of the nickel mesh catalyst coating of the alkaline electrolytic cell provided in the present invention is high, so that the spraying process has a lower spraying cost; in addition, the nickel mesh catalyst coating prepared by the spraying process has good thickness uniformity and strong bonding with the nickel mesh.

[0016] Preferably, the nickel mesh in step (1) is a sandblasted nickel mesh.

[0017] Preferably, the roughness of the sandblasted nickel mesh is Sa3 level.

[0018] The roughness of Sa3 level in the present invention corresponds to a Ra value of 0.8~2.5μm, for example, it can be 0.8μm, 1m, 1.2μm, 1.4μm, 1.6μm, 1.8μm, 2μm, 2.2μm, 2.4μm or 2.5μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the method for preparing the sandblasted nickel mesh comprises: leveling an initial nickel mesh and then sandblasting it.

[0020] Preferably, the initial nickel mesh comprises a woven nickel mesh.

[0021] Preferably, the leveling method includes using a leveling machine to level the initial nickel mesh.

[0022] Preferably, the flatness of the flattened nickel mesh obtained after flattening is not higher than 5 mm, for example, it can be 5 mm, 4.5 mm, 4 mm, 3.5 mm, 3 mm, 2.5 mm, 2 mm, 1.5 mm, 1 mm or 0.5 mm, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, cleaning and drying are performed sequentially between the leveling and the sandblasting.

[0024] Preferably, the cleaning is performed on a nickel mesh degreasing cleaning line, and the flattened nickel mesh passes through a cleaning tank containing a cleaning agent.

[0025] Preferably, the drying temperature is 100-120°C, for example, it may be 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C, 118°C or 120°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the sandblasting uses white corundum grit of 60-90 mesh, for example, it can be 60 mesh, 62 mesh, 65 mesh, 67 mesh, 70 mesh, 72 mesh, 75 mesh, 77 mesh, 80 mesh, 82 mesh, 85 mesh, 87 mesh or 90 mesh, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the pressure of the sandblasting is 0.5-0.7 MPa, and the time for each part of the nickel mesh to pass through the effective sandblasting area during the sandblasting is 10-15 s.

[0028] The sandblasting pressure of the present invention is 0.5~0.7MPa, for example, it can be 0.5MPa, 0.52MPa, 0.54MPa, 0.56MPa, 0.58MPa, 0.6MPa, 0.62MPa, 0.64MPa, 0.66MPa, 0.68MPa or 0.7MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] The time for each part of the nickel mesh to pass through the effective sandblasting area in the sandblasting of the present invention is 10 to 15 seconds, for example, it can be 10 seconds, 10.5 seconds, 11 seconds, 11.5 seconds, 12 seconds, 12.5 seconds, 13 seconds, 13.5 seconds, 14 seconds, 14.5 seconds or 15 seconds, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; for the entire nickel mesh of 1.8m×1.8m, the total sandblasting time is 6 to 10 minutes, for example, it can be 6 minutes, 6.5 minutes, 7 minutes, 7.5 minutes, 8 minutes, 8.5 minutes, 9 minutes, 9.5 minutes or 10 minutes, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the time interval between the sandblasting and the first powder spraying in step (1) is not longer than 4 hours, for example, it can be 4 hours, 3.8 hours, 3.6 hours, 3.4 hours, 3.2 hours, 3 hours, 2.8 hours, 2.6 hours, 2.4 hours, 2.2 hours, 2 hours, 1.8 hours, 1.6 hours, 1.4 hours, 1.2 hours or 1 hour, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] Preferably, the set angle θ1 in step (1) is 5 to 30 degrees, for example, it can be 5 degrees, 7 degrees, 10 degrees, 12 degrees, 15 degrees, 17 degrees, 20 degrees, 22 degrees, 25 degrees, 27 degrees or 30 degrees, but is not limited to the listed values. Other values ​​not listed in the numerical range are also applicable, preferably 10 to 20 degrees.

[0032] Preferably, in step (1), the height between the spray gun and the nickel mesh in the first powder spraying is h×cosθ1, and h is 80~150mm, for example, it can be 80mm, 85mm, 90mm, 95mm, 100mm, 105mm, 110mm, 120mm, 130mm, 140mm or 150mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, in step (1), the powder feeding speed of the spray gun in the first powder spraying is 60-100 g / min, for example, 60 g / min, 65 g / min, 70 g / min, 75 g / min, 80 g / min, 85 g / min, 90 g / min, 95 g / min or 100 g / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] Preferably, in step (1), the moving speed of the spray gun in the first powder spraying is 0.5-1 m / s, for example, 0.5 m / s, 0.6 m / s, 0.7 m / s, 0.8 m / s, 0.9 m / s or 1 m / s, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; for a whole nickel mesh of 1.8 m×1.8 m, the total sandblasting time is 15-30 min.

[0035] The time of the first powder spraying in the present invention can be obtained according to the size of the nickel mesh and the speed of the gun.

[0036] Preferably, the powder sprayed by the first powder spraying in step (1) includes any one of nickel-aluminum mixed powder, nickel-coated aluminum powder, aluminum-coated nickel powder or nickel-aluminum alloy powder, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of nickel-aluminum mixed powder and nickel-coated aluminum powder, a combination of nickel-coated aluminum powder and aluminum-coated nickel powder, a combination of aluminum-coated nickel powder and nickel-aluminum alloy powder, or a combination of nickel-aluminum mixed powder, nickel-coated aluminum powder and aluminum-coated nickel powder.

[0037] Preferably, in step (2), the setting angle θ2=-θ1.

[0038] Preferably, the set angle θ2 in step (2) is -5 to -30 degrees, for example, it can be -5 degrees, -10 degrees, -15 degrees, -20 degrees, -25 degrees or -30 degrees, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably -10 to -20 degrees.

[0039] Preferably, in step (2), the height between the spray gun and the nickel mesh in the second powder spraying is h×cos(θ1+θ2), and h is 80~150mm, for example, it can be 80mm, 90mm, 100mm, 110mm, 120mm, 130mm, 140mm or 150mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0040] Preferably, in step (2), the powder feeding speed of the spray gun in the second powder spraying is 60-100 g / min, for example, 60 g / min, 65 g / min, 70 g / min, 75 g / min, 80 g / min, 85 g / min, 90 g / min, 95 g / min or 100 g / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] Preferably, in step (2), the moving speed of the spray gun in the second powder spraying is 0.5-1 m / s, for example, 0.5 m / s, 0.6 m / s, 0.7 m / s, 0.8 m / s, 0.9 m / s or 1 m / s, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; for a whole nickel mesh of 1.8 m×1.8 m, the total sandblasting time is 15-30 min.

[0042] Preferably, the powder sprayed by the second powder spraying in step (2) includes any one of nickel-aluminum mixed powder, nickel-coated aluminum powder, aluminum-coated nickel powder or nickel-aluminum alloy powder, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of nickel-aluminum mixed powder and nickel-coated aluminum powder, a combination of nickel-coated aluminum powder and aluminum-coated nickel powder, a combination of aluminum-coated nickel powder and nickel-aluminum alloy powder, or a combination of nickel-aluminum mixed powder, nickel-coated aluminum powder and aluminum-coated nickel powder.

[0043] As a preferred technical solution of the spraying process of the present invention, the spraying process includes:

[0044] (1) The woven nickel mesh is flattened to obtain a flattened nickel mesh with a flatness of no more than 5 mm, and then the mesh is cleaned and dried in sequence and then sandblasted. The pressure of the sandblasting is 0.5-0.7 MPa, and the time for each part of the nickel mesh to pass through the effective sandblasting area is 10-15 seconds. A sandblasted nickel mesh with a roughness of Sa3 is obtained, and two sheets of the obtained sandblasted nickel mesh are stacked and then subjected to the first powder spraying;

[0045] The spray direction of the spray gun in the first powder spraying maintains the same angle with the warp and weft of the nickel mesh on the top layer, and the angle with the normal direction of the plane of the nickel mesh on the top layer is a set angle θ1, θ1 is 5-30 degrees; the height of the spray gun from the nickel mesh is h×cosθ1, h is 80-150 mm, the powder feeding speed of the spray gun is 60-100 g / min, and the moving speed of the spray gun is 0.5-1 m / s;

[0046] (2) After the positions of the two nickel meshes are swapped, the spray direction of the spray gun is rotated to a set angle θ2 with the normal direction of the nickel mesh plane as the axis, and then a second powder spraying is performed to obtain a nickel mesh catalyst coating;

[0047] θ2 is -θ1, and the height between the spray gun and the nickel mesh in the second powder spraying is h×cosθ2, wherein h is 80-150 mm, the powder feeding speed of the spray gun is 60-100 g / min, and the moving speed of the spray gun is 0.5-1 m / s.

[0048] In a second aspect, the present invention provides a nickel mesh catalyst coating for an alkaline electrolytic cell, wherein the nickel mesh catalyst coating is obtained by the spraying process described in the first aspect.

[0049] In a third aspect, the present invention provides an alkaline electrolytic cell, comprising the nickel mesh catalyst coating according to the second aspect.

[0050] In a fourth aspect, the present invention provides an application of the alkaline electrolyzer described in the third aspect, wherein the alkaline electrolyzer is used for producing hydrogen by electrolyzing water in an alkaline environment.

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] The powder utilization rate of the spraying process of the nickel mesh catalyst coating of the alkaline electrolytic cell provided in the present invention is high, so that the spraying process has a lower spraying cost; in addition, the nickel mesh catalyst coating prepared by the spraying process has good thickness uniformity and strong bonding with the nickel mesh. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 Schematic diagram of the spray direction of the spray gun and the position of the woven nickel mesh in the spraying process of Example 1.

[0054] Figure 2 Schematic diagram of the spray direction of the spray gun and the position of the woven nickel mesh in the spraying process of Comparative Example 1.

[0055] Among them, 1-woven nickel mesh; 2-spray gun. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0057] Example 1

[0058] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, the spraying process comprising:

[0059] (1) If Figure 1 As shown, the woven nickel mesh 1 is flattened to obtain a flattened nickel mesh with a flatness of 3 mm, which is then cleaned and dried in sequence and then sandblasted. The pressure of the sandblasting is 0.6 MPa, and the time for each part of the nickel mesh to pass through the effective sandblasting area during the sandblasting is 12 seconds. A sandblasted nickel mesh with a roughness of Sa3 is obtained, and two sheets of the obtained sandblasted nickel mesh are stacked and then subjected to the first powder spraying;

[0060] The spray direction of the spray gun 2 in the first powder spraying maintains the same angle with the warp and weft of the nickel mesh on the top layer, and the angle with the normal direction of the nickel mesh plane on the top layer is a set angle θ1, θ1 is 20 degrees; the height of the spray gun 2 from the nickel mesh is h×cosθ1, h is 120 mm, the powder feeding speed of the spray gun 2 is 80 g / min, and the moving speed of the spray gun 2 is 0.8 m / s;

[0061] (2) After the positions of the two nickel meshes are swapped, the spray direction of the spray gun 2 is rotated to a set angle θ2 with the normal direction of the nickel mesh plane as the axis, and then a second powder spraying is performed to obtain a nickel mesh catalyst coating;

[0062] θ2 is -θ1 (-20 degrees), the height between the spray gun 2 and the nickel mesh in the second powder spraying is h×cosθ2, where h is 120 mm, the powder feeding speed of the spray gun 2 is 80 g / min, and the moving speed of the spray gun 2 is 0.8 m / s.

[0063] Example 2

[0064] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, the spraying process comprising:

[0065] (1) The woven nickel mesh 1 is flattened to obtain a flattened nickel mesh with a flatness of 3 mm, and then the mesh is cleaned and dried in sequence and then sandblasted. The sandblasting pressure is 0.7 MPa, and the time for each part of the nickel mesh to pass through the effective sandblasting area during the sandblasting is 10 s. A sandblasted nickel mesh with a roughness of Sa3 is obtained. Two sheets of the obtained sandblasted nickel mesh are stacked and then subjected to the first powder spraying;

[0066] The spray direction of the spray gun 2 in the first powder spraying maintains the same angle with the warp and weft of the nickel mesh on the top layer, and the angle with the normal direction of the plane of the nickel mesh on the top layer is a set angle θ1, θ1 is 10 degrees; the height of the spray gun 2 from the nickel mesh is h×cosθ1, h is 150mm, the powder feeding speed of the spray gun 2 is 100g / min, and the moving speed of the spray gun 2 is 1m / s;

[0067] (2) After the positions of the two nickel meshes are swapped, the spray direction of the spray gun 2 is rotated to a set angle θ2 with the normal direction of the nickel mesh plane as the axis, and then a second powder spraying is performed to obtain a nickel mesh catalyst coating;

[0068] θ2 is -θ1 (-10 degrees), the height between the spray gun 2 and the nickel mesh in the second powder spraying is h×cosθ2, where h is 150 mm, the powder feeding speed of the spray gun 2 is 100 g / min, and the moving speed of the spray gun 2 is 1 m / s.

[0069] Example 3

[0070] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, the spraying process comprising:

[0071] (1) The woven nickel mesh 1 is flattened to obtain a flattened nickel mesh with a flatness of 3 mm, and then the mesh is cleaned and dried in sequence and then sandblasted. The sandblasting pressure is 0.5 MPa, and the time for each part of the nickel mesh to pass through the effective sandblasting area during the sandblasting is 15 seconds. A sandblasted nickel mesh with a roughness of Sa3 is obtained, and two sheets of the obtained sandblasted nickel mesh are stacked and then subjected to the first powder spraying;

[0072] The spray direction of the spray gun 2 in the first powder spraying maintains the same angle with the warp and weft of the nickel mesh on the top layer, and the angle with the normal direction of the plane of the nickel mesh on the top layer is a set angle θ1, θ1 is 30 degrees; the height of the spray gun 2 from the nickel mesh is h×cosθ1, h is 80 mm, the powder feeding speed of the spray gun 2 is 60 g / min, and the moving speed of the spray gun 2 is 0.6 m / s;

[0073] (2) After the positions of the two nickel meshes are swapped, the spray direction of the spray gun 2 is rotated to a set angle θ2 with the normal direction of the nickel mesh plane as the axis, and then a second powder spraying is performed to obtain a nickel mesh catalyst coating;

[0074] θ2 is -θ1 (-30 degrees), the height between the spray gun 2 and the nickel mesh in the second powder spraying is h×cosθ2, where h is 80 mm, the powder feeding speed of the spray gun 2 is 60 g / min, and the moving speed of the spray gun 2 is 0.6 m / s.

[0075] Example 4

[0076] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the angle θ1 is set to 2 degrees in step (1).

[0077] Example 5

[0078] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the angle θ1 is set to 40 degrees in step (1).

[0079] Example 6

[0080] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the height of the spray gun 2 in the first powder spraying from the nickel mesh is h×cosθ1, and h is 180 mm.

[0081] Example 7

[0082] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the powder feeding speed of the spray gun 2 in step (1) is 50 g / min.

[0083] Example 8

[0084] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the powder feeding speed of the spray gun 2 in step (1) is 120 g / min.

[0085] Example 9

[0086] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the angle θ2 is set to -2 degrees in step (2).

[0087] Example 10

[0088] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the angle θ2 is set to -40 degrees in step (2).

[0089] Embodiment 11

[0090] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the height of the spray gun 2 from the nickel mesh in the second powder spraying in step (2) is h×cosθ2, and h is 180 mm.

[0091] Example 12

[0092] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the powder feeding speed of the spray gun 2 in step (2) is 40 g / min.

[0093] Embodiment 13

[0094] This embodiment provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, which is the same as that of Embodiment 1 except that the powder feeding speed of the spray gun 2 in step (2) is 120 g / min.

[0095] Comparative Example 1

[0096] This comparative example provides a spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, and the spraying process is as follows: Figure 2As shown, the substrate sandblasting includes two steps: pretreatment and spraying; the first step of pretreatment is: through a typical sandblasting process, the parameters of the sandblasting process are 50 mesh corundum sand, the sandblasting pressure is 0.35 MPa, and the time for the nickel mesh to pass through the effective sandblasting area is 12 s; the second step of the spraying process is: leveling the woven nickel mesh to obtain a leveled nickel mesh with a flatness of 35 mm, and then cleaning and drying it in turn before sandblasting, the sandblasting pressure is 0.35 MPa, the grit mesh is 50 mesh, and the time for the nickel mesh to pass through the effective sandblasting area is 12 s, and a sandblasted nickel with a roughness of Sa3 level is obtained; then, a single nickel mesh is powdered, and the preset thickness is achieved by one spraying. The spray direction of the spray gun is the normal direction of the nickel mesh plane, and the height from the nickel mesh is h, wherein h is 120 mm, the powder feeding speed of the spray gun is 80 g / min, and the gun travel speed is 0.4 m / s.

[0097] The woven nickel mesh 1 with a nickel mesh catalyst coating was prepared by the spraying process in the above-mentioned embodiment and the comparative example. The weight gain rate of the woven nickel mesh 1 was obtained by weighing as shown in Table 1, the mass of the consumed powder was recorded as shown in Table 1, and the powder utilization rate was calculated by the weight gain rate and the mass of the consumed powder as shown in Table 1; then the nickel mesh catalyst coating was subjected to an alkali boiling experiment, and the alkali boiling experiment was as follows: the woven nickel mesh 1 with the nickel mesh catalyst coating was cut into 3 pieces of size 3×3 cm, and then placed in a flask containing 30% KOH solution, placed in an ultrasonic water bath heater, and the water bath temperature was set to 70°C. After 24 hours, the sample was taken out and weighed, and the weight loss rate was calculated. The alkali boiling weight loss rate obtained by testing is shown in Table 1.

[0098] Table 1

[0099]

[0100] From Table 1, we can get:

[0101] (1) The spraying process of the nickel mesh catalyst coating of the alkaline electrolytic cell provided in Examples 1 to 3 of the present invention has a high weight gain rate, consumes less powder and has a high powder utilization rate. The woven nickel mesh 1 with the nickel mesh catalyst coating prepared by the spraying process has a low alkali boiling weight loss rate;

[0102] (2) By comparing Example 1 with Examples 4 and 5, it can be seen that the setting angle θ1 in step (1) of the present invention will affect the performance of the spraying process and the performance of the prepared woven nickel mesh 1 with a nickel mesh catalyst coating; when the setting angle θ1 is too small, the weight gain rate will be reduced, the powder consumption will be more, the powder utilization rate will be lower, and the alkali boiling weight loss rate will be higher. This is because the overlapping part of the two spraying areas is large, the thickness at the thickest part of the top is large, the internal stress is reduced, the overall thickness distribution is poor, and the bonding between the coating and the substrate is reduced; when the setting angle θ1 is too large, the weight gain rate will be reduced, the powder consumption will be more, the powder utilization rate will be lower, and the alkali boiling weight loss rate will be higher. This is because the plasma arc spot is overly elongated into an ellipse, and the flying distance difference of the particles in the plasma flow is too large, resulting in a decrease in adhesion quality;

[0103] (3) By comparing Example 1 with Example 6, it can be seen that the height of the spray gun 2 from the nickel mesh in the first powder spraying in step (1) of the present invention will affect the performance of the spraying process and the performance of the prepared woven nickel mesh 1 with a nickel mesh catalyst coating; when the height is too high, it will lead to a lower weight gain rate, a larger powder consumption, a lower powder utilization rate and a higher alkali boiling weight loss rate. This is because the plasma flow temperature is reduced and the temperature of the particles when they hit the substrate is insufficient, resulting in a decrease in both deposition rate and adhesion;

[0104] (4) By comparing Example 1 with Examples 7 and 8, it can be seen that the powder feeding speed of the spray gun 2 in step (1) of the present invention will affect the performance of the spraying process and the performance of the prepared woven nickel mesh 1 with a nickel mesh catalyst coating; when the powder feeding speed of the spray gun 2 is too small, the weight gain rate will be small, the production efficiency will be low, and the energy consumption will be high. This is because there is less powder, the powder application speed is slow, and the coating is thin; when the powder feeding speed of the spray gun 2 is too large, the powder melting degree will decrease, affecting the deposition rate and adhesion rate, the powder consumption will increase, the powder utilization rate will decrease, and the alkali boiling weight loss rate will decrease. This is because when the powder feeding speed is too large, although the powder application speed is fast, it will cause the powder melting degree to decrease, and many powders cannot be combined or are poorly combined, resulting in low powder utilization and increased alkali boiling weight loss;

[0105] (5) By comparing Example 1 with Examples 9 and 10, it can be seen that the setting angle θ2 in step (2) of the present invention will affect the performance of the spraying process and the performance of the prepared woven nickel mesh 1 with a nickel mesh catalyst coating; when the absolute value of the setting angle θ2 is too small, the weight gain rate will be reduced, the powder consumption will be more, the powder utilization rate will be lower, and the alkali boiling weight loss rate will be higher. This is because the overlapping part of the two spraying areas is large, the thickness at the thickest part of the top is large, the internal stress is reduced, the overall thickness distribution is poor, and the bonding between the coating and the substrate is reduced; when the absolute value of the setting angle θ2 is too large, the weight gain rate will be reduced, the powder consumption will be more, the powder utilization rate will be lower, and the alkali boiling weight loss rate will be higher. This is because the plasma arc spot is overly elongated into an ellipse, and the flying distance difference of the particles in the plasma flow is too large, resulting in a decrease in adhesion quality;

[0106] (6) By comparing Example 1 with Example 11, it can be seen that the height of the spray gun 2 from the nickel mesh in the second powder spraying in step (2) of the present invention will affect the performance of the spraying process and the performance of the prepared woven nickel mesh 1 with a nickel mesh catalyst coating; when the height is too high, it will lead to a lower weight gain rate, a larger powder consumption, a lower powder utilization rate and a higher alkali boiling weight loss rate. This is because the plasma flow temperature is reduced and the temperature of the particles when they hit the substrate is insufficient, resulting in a decrease in both deposition rate and adhesion;

[0107] (7) By comparing Example 1 with Examples 12 and 13, it can be seen that the powder feeding speed of the spray gun 2 in step (2) of the present invention affects the performance of the spraying process and the performance of the prepared woven nickel mesh 1 with a nickel mesh catalyst coating; when the powder feeding speed of the spray gun 2 is too small, the weight gain rate will decrease. This is because when the powder feeding speed is too small, the powder loading speed is small and the efficiency is low; when the powder feeding speed of the spray gun 2 is too large, the powder consumption will increase, the powder utilization rate will decrease, and the alkali boiling weight loss rate will increase. This is because although the powder loading speed is fast, it will cause the powder melting degree to decrease, and many powders cannot be combined or are poorly combined, resulting in low powder utilization and increased alkali boiling weight loss;

[0108] (8) By comparing Example 1 with Comparative Example 1, it can be seen that the spray direction of the spray gun 2 in the first powder spraying of the present invention maintains the same angle with the warp and weft of the nickel mesh on the top layer, and the angle with the normal direction of the plane of the nickel mesh on the top layer is a set angle θ1, so the projection area of ​​the hole area perpendicular to the spraying direction is also smaller than the area of ​​the mesh, which reduces the amount of powder leaking through the mesh and improves the powder utilization rate; during the first powder spraying of the present invention, the top nickel mesh is mainly sprayed, but part of the powder leaking from the mesh of the top nickel mesh will be received by the top nickel mesh, thereby reducing the waste of powder and improving the powder application rate; after the first powder spraying is completed, the two nickel meshes are exchanged and the original The bottom nickel mesh is first placed on top, and then the spray direction of the spray gun 2 is rotated θ2 with the normal direction of the top nickel mesh plane as the axis to be a new spray direction, and the second powder spraying is performed to reach the preset powder application amount; in the present invention, the directions of the first powder spraying and the second powder spraying do not completely overlap, the thickness at the thickest part of the top is reduced, the internal stress is reduced, the overall thickness distribution is relatively more uniform, the proportion of the area with moderate thickness is increased, and the bonding force between the coating and the nickel mesh is enhanced; the powder utilization rate of the spraying process of the nickel mesh catalyst coating provided in the present invention is high, so that the spraying process has a lower spraying cost; in addition, the thickness uniformity of the nickel mesh catalyst coating prepared by the spraying process is good and the bonding force with the nickel mesh is strong.

[0109] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A spraying process for a nickel mesh catalyst coating of an alkaline electrolytic cell, characterized in that: The spraying process includes: (1) After stacking two nickel meshes, a first powder spraying is performed, wherein the spraying direction of the spray gun in the first powder spraying maintains the same angle with the warp and weft of the nickel mesh of the top layer, and the angle with the normal direction of the plane of the nickel mesh of the top layer is a set angle θ1; (2) After the positions of the two nickel meshes are swapped, the spray direction of the spray gun is rotated to a set angle θ2 with the normal direction of the nickel mesh plane as the axis, and then a second powder spraying is performed to obtain a nickel mesh catalyst coating.

2. The spraying process according to claim 1, characterized in that: The nickel mesh in step (1) is a sandblasted nickel mesh; The roughness of the sandblasted nickel mesh is Sa3 level; The method for preparing the sandblasted nickel mesh comprises: leveling and then sandblasting the initial nickel mesh; The initial nickel mesh comprises a woven nickel mesh; The flatness of the flattened nickel mesh obtained after the flattening is not higher than 5 mm; The leveling and sandblasting also include cleaning and drying in sequence; The pressure of the sandblasting is 0.5-0.7 MPa, and the time for each part of the nickel mesh to pass through the effective sandblasting area during the sandblasting is 10-15 seconds; The time interval between the sandblasting and the first powder spraying in step (1) is no longer than 4 hours.

3. The spraying process according to claim 1, characterized in that: The setting angle θ1 in step (1) is 5 to 30 degrees.

4. The spraying process according to claim 1, characterized in that: Step (1) In the first powder spraying, the height between the spray gun and the nickel mesh is h×cosθ1, where h is 80-150 mm; Step (1) The powder feeding speed of the spray gun in the first powder spraying is 60-100 g / min; Step (1) The movement speed of the spray gun in the first powder spraying is 0.5-1 m / s; The powder sprayed by the first powder spraying in step (1) includes any one of nickel-aluminum mixed powder, nickel-coated aluminum powder, aluminum-coated nickel powder or nickel-aluminum alloy powder, or a combination of at least two thereof.

5. The spraying process according to claim 1, characterized in that: Step (2) wherein the angle θ2 is set to -θ1; The setting angle θ2 in step (2) is -5 to -30 degrees.

6. The spraying process according to claim 1, characterized in that: Step (2) In the second powder spraying, the height between the spray gun and the nickel mesh is h×cosθ2, where h is 80-150 mm; Step (2) The powder feeding speed of the spray gun in the second powder spraying is 60-100 g / min; Step (2) The moving speed of the spray gun in the second powder spraying is 0.5-1 m / s; The powder sprayed by the second powder spraying in step (2) includes any one of nickel-aluminum mixed powder, nickel-coated aluminum powder, aluminum-coated nickel powder or nickel-aluminum alloy powder, or a combination of at least two thereof.

7. The spraying process according to any one of claims 1 to 6, characterized in that: The spraying process includes: (1) The woven nickel mesh is flattened to obtain a flattened nickel mesh with a flatness of no more than 5 mm, and then the mesh is cleaned and dried in sequence and then sandblasted. The pressure of the sandblasting is 0.5-0.7 MPa. The time for each part of the nickel mesh to pass through the effective sandblasting area during the sandblasting is 10-15 seconds. A sandblasted nickel mesh with a roughness of Sa3 is obtained. Two sheets of the obtained sandblasted nickel mesh are stacked and then subjected to the first powder spraying; The spray direction of the spray gun in the first powder spraying maintains the same angle with the warp and weft of the nickel mesh on the top layer, and the angle with the normal direction of the nickel mesh plane on the top layer is a set angle θ1, θ1 is 5-30 degrees; the height of the spray gun from the nickel mesh is h×cosθ1, h is 80-150 mm, the powder feeding speed of the spray gun is 60-100 g / min, and the moving speed of the spray gun is 0.5-1 m / s; (2) After the positions of the two nickel meshes are swapped, the spray direction of the spray gun is rotated to a set angle θ2 with the normal direction of the nickel mesh plane as the axis, and then a second powder spraying is performed to obtain a nickel mesh catalyst coating; θ2 is -θ1, and the height between the spray gun and the nickel mesh in the second powder spraying is h×cosθ2, wherein h is 80-150 mm, the powder feeding speed of the spray gun is 60-100 g / min, and the moving speed of the spray gun is 0.5-1 m / s.

8. A nickel mesh catalyst coating for an alkaline electrolytic cell, characterized in that: The nickel mesh catalyst coating is obtained by the spraying process described in any one of claims 1 to 7.

9. An alkaline electrolytic cell, characterized in that: The alkaline electrolytic cell comprises the nickel mesh catalyst coating of claim 8.

10. Use of the alkaline electrolytic cell according to claim 9, characterized in that: The alkaline electrolyzer is used for producing hydrogen by electrolyzing water in an alkaline environment.

Citation Information

Patent Citations

  • Spraying device for nickel-aluminum coating on surface of silk screen

    CN116328993A

  • Porous catalytic electrode for electrolyzing water, preparation method of porous catalytic electrode and electrolyzing device

    CN118756192A

  • Nickel wire mesh applied to hydrogen production electrolytic cell

    CN217677802U

  • FR2214223A1

  • Wear resistant screen

    US20060210721A1