Surface cladding process for inner hole of large thin-walled cylinder type steering tube forge piece
Through the laser cladding process, combined with powder composition ratio and parameter control, the problem of unstable cylindricality during operation of the inner hole of the steering tube is solved, and the effect of high strength and corrosion resistance is achieved, extending the service life of the steering tube.
Patent Information
- Application Number
- CN202410980198.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-26
AI Technical Summary
During operation, the inner hole of the steering pipe is prone to deformation due to friction and torsional forces, resulting in unstable cylindricality, affecting the coordination with the bearing, and the prior art is difficult to avoid thermal deformation and cracks while ensuring high strength.
Using laser cladding technology, the powder components are matched with the steering tube forging substrate by reasonably proportionalizing the powder components, and the output power, scanning speed and powder output are controlled to achieve spiral uniform cladding, ensuring high strength, corrosion resistance and stability of cylindricality sex.
It realizes high strength, corrosion resistance and wear resistance of the inner bore surface of the steering tube, while maintaining the stability of cylindricality, improving the stability and life of the steering tube, and avoiding the risks of thermal deformation and cracks.
Smart Images

Figure CN119020773A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging. By laser cladding the inner hole surface of the steering tube, the inner hole surface is not only high-strength, corrosion-resistant and wear-resistant, but also has stable cylindricity, thereby improving the service stability and service life of the steering tube. Background Art
[0002] The steering tube is mainly used in the lateral propulsion system of ships. The inner hole of the steering tube is matched with a high-precision bearing assembly, and the flange is connected to the servo shaft. During operation, the steering tube needs to rotate at a constant speed and bear the friction with the bearing and the torsional force of the servo shaft. To ensure that under the action of continuous torsional force, the steering tube substrate must have a strength of more than 750MPa. At the same time, the precision of the bearing assembly is extremely high. After the inner hole of the steering tube is matched with it, the cylindricality must be controlled below 0.02mm, and this value must remain stable. If the inner hole is deformed after long-term operation, it will interfere with the bearing and cause "stuck" phenomenon. Therefore, the inner hole of the steering tube must be strengthened. After the inner hole is laser melted, the surface hardness of the inner hole can reach at least 450HB, which has high strength characteristics. In addition, after the iron-based or nickel-based material powder is melted, the powder particle size is evenly and finely stacked, the density is excellent, and it can continuously play a role in corrosion resistance. Summary of the invention
[0003] Design purpose: To avoid the shortcomings of the background technology, a surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging is designed to achieve high strength, corrosion resistance, and wear resistance through laser cladding of the inner hole surface of the steering tube, while also having a stable cylindricity, thereby improving the service stability and life of the steering tube.
[0004] Design scheme: In order to achieve the design purpose of the present invention. The present invention adopts the composition ratio of the powder for laser cladding, and the relationship between the composition ratio and the basic material of the steering tube forging, and according to the actual working conditions of the steering tube forging, on the premise of matching the powder composition ratio and the steering tube forging base material, the laser cladding parameters are set to ensure that there are no defects such as cracks on the surface after cladding.
[0005] Laser melting and covering is a process that outputs a certain amount of specific powder, melts it instantly with laser, and adheres it to the surface of the workpiece in an orderly manner. It is a surface modification technology with strong metallurgical bonding and high density. It can mix the corresponding powder according to the surface working conditions and has a high degree of application. At the same time, laser cladding has a small heat-affected zone and has obvious advantages over electric welding, electroplating and other methods in the repair of some precision products. It is a new process technology with market prospects.
[0006] The adaptability and size of the steering tube are determined by the power of the lateral propulsion system. The current mainstream sizes are as follows: Figure 1 shown.
[0007] Corresponding relationship between steering tube inner hole diameter, inner hole effective section length, total length and strength Table of the relationship between the tensile strength of the substrate and the composition of the powder used for laser cladding Compared with the background technology, the present invention has the following advantages: first, since the wall thickness of the steering tube forging is relatively thin (maximum 55mm), the present invention adopts laser cladding, which does not require heating of the substrate and can be implemented at room temperature. The thermal impact is extremely small, and the inner hole of the steering tube will not be thermally deformed, which can fully ensure that the cylindricity still meets the requirement of less than 0.05mm after cladding. At the same time, spiral cladding is adopted to make the stress distribution uniform. Second, steering tubes of different materials and different strength conditions are subdivided and allocated with corresponding cladding powders, so that the compatibility between the substrate and the cladding powder is stronger, avoiding the risk of cracks in the cladding layer. Third, through precise control of output power, scanning speed, powder output and cladding thickness, it can be ensured that the cladding layer adheres to the workpiece surface uniformly, densely and with stronger bonding force, so that the steering tube can fully achieve the characteristics of high strength and high corrosion and wear resistance, and further ensure the service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 This is a schematic diagram of the current mainstream specifications and dimensions of steering tubes.
[0009] Figure 2 It is a schematic diagram of the implementation of the present invention. DETAILED DESCRIPTION
[0010] Refer to the attached Figure 1 and 2 A surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging. Place the steering tube on a horizontal lathe, adjust the level by supporting the bracket and the claws, and use a dial indicator to check that the cylindricity of the steering tube during rotation is less than 0.05mm; Laser cladding system equipment, the robot arm bracket is fixed on the horizontal machine tool beam, and the robot arm joint can flexibly penetrate into the inner hole of the steering tube; the device is as follows Figure 2 : According to the different inner hole diameters of the special tubes and the base material, the output power and machine speed of the cladding equipment are reasonably matched; see the following table for details: After determining the output power and machine tool rotation speed, the scanning speed of the cladding nozzle and the powder output amount need to be set during cladding; see the table below for details: Continuous cladding: The inner hole is clad continuously from the inside to the outside, and the cladding layer is distributed in a spiral shape with uniform thickness and width until the entire inner hole cladding surface is completely clad.
[0011] After the single-layer cladding is completed, the cladding layer of the inner hole is machined to remove 0.2mm of the cladding layer to make the inner hole smooth and clean.
[0012] Example 1: A surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging. When the inner hole diameter of the steering tube is 300 mm and the substrate is 42CrMo, the output power of the cladding equipment is 900 Kwh, the machine tool speed is 1.0 rpm, the scanning speed of the cladding nozzle is 6 mm / s, the powder output is 12 g / min, the single-layer cladding thickness is 0.4 mm, and the single-pass cladding width is 3 mm.
[0013] Example 2: A surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging. When the inner hole diameter of the steering tube is 400 mm and the substrate is 42CrMo, the output power of the cladding equipment is 1000 Kwh, the machine tool speed is 0.8 rpm, the scanning speed of the cladding nozzle is 6 mm / s, the powder output is 12 g / min, the single-layer cladding thickness is 0.4 mm, and the single-pass cladding width is 3 mm.
[0014] Example 3: A surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging. When the inner hole diameter of the steering tube is 450 mm and the substrate is 34CrNiMo6, the output power of the cladding equipment is 1300 Kwh, the machine tool speed is 0.6 rpm, the scanning speed of the cladding nozzle is 10 mm / s, and the powder output is 20 g / min. The single-layer cladding thickness is 0.6 mm and the single-pass cladding width is 3 mm.
[0015] Example 4: A surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging. When the inner hole diameter of the steering tube is 500 mm and the substrate is 34CrNiMo6, the output power of the cladding equipment is 1500 Kwh, the machine tool speed is 0.4 rpm, the scanning speed of the cladding nozzle is 10 mm / s, the powder output is 20 g / min, the single-layer cladding thickness is 0.6 mm, and the single-pass cladding width is 3 mm.
[0016] It should be understood that although the above embodiments provide a relatively detailed textual description of the design ideas of the present invention, these textual descriptions are only simple textual descriptions of the design ideas of the present invention, rather than limitations on the design ideas of the present invention. Any combination, addition or modification that does not exceed the design ideas of the present invention shall fall within the protection scope of the present invention.
Claims
1. A surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging, characterized in that: 1) Place the steering tube on a horizontal lathe, adjust the level by supporting the bracket and the claws, and use a dial indicator to check that the cylindricality of the steering tube is less than 0.05mm during rotation; 2) The mechanical arm bracket in the laser cladding system equipment is fixed on the horizontal machine tool beam, and the mechanical arm joint can flexibly penetrate into the inner hole of the steering tube; 3) When the inner diameter of the steering tube is 300-500mm and the base material is 42CrMo or 34CrNiMo6, the output power of the cladding equipment is 900-1500Kwh and the machine speed is 1.0-0.4 rpm; 4) After determining the output power and machine tool rotation speed, the scanning speed of the cladding nozzle is 6-10mm / s, the powder output is 12-20 g / min, the single-layer cladding thickness is 0.4-0.6mm, and the single-pass cladding width is 3mm; 5) Continuous cladding: The inner hole is clad continuously from the inside to the outside. The cladding layer is distributed in a spiral shape with uniform thickness and width until the entire inner hole cladding surface is completely clad.
2. The surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging according to claim 1 is characterized by: When the inner diameter of the steering tube is 300mm and the substrate is 42CrMo, the output power of the cladding equipment is 900Kwh, the machine speed is 1.0 rpm, the scanning speed of the cladding nozzle is 6mm / s, the powder output is 12g / min, the single-layer cladding thickness is 0.4mm, and the single-pass cladding width is 3mm.
3. The surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging according to claim 1 is characterized by: When the inner diameter of the steering tube is 400mm and the substrate is 42CrMo, the output power of the cladding equipment is 1000Kwh, the machine speed is 0.8 rpm, the scanning speed of the cladding nozzle is 6mm / s, the powder output is 12g / min, the single-layer cladding thickness is 0.4mm, and the single-pass cladding width is 3mm.
4. The surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging according to claim 1 is characterized by: When the inner diameter of the steering tube is 450mm and the substrate is 34CrNiMo6, the output power of the cladding equipment is 1300Kwh, the machine tool speed is 0.6 rpm, the scanning speed of the cladding nozzle is 10mm / s, the powder output is 20g / min, the single-layer cladding thickness is 0.6mm, and the single-pass cladding width is 3mm.
5. The surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging according to claim 1 is characterized by: When the inner diameter of the steering tube is 500mm and the substrate is 34CrNiMo6, the output power of the cladding equipment is 1500Kwh, the machine tool speed is 0.4 rpm, the scanning speed of the cladding nozzle is 10mm / s, the powder output is 20g / min, the single-layer cladding thickness is 0.6mm, and the single-pass cladding width is 3mm.
6. The surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging according to claim 1 is characterized by: When the substrate is 42CrMo, the powder composition for laser cladding in the laser cladding system equipment is Ni87.75%, C0.25%, Si3.0%, B1.0%, Fe2.4%, Cr5.6% in weight percentage, and the total amount error is ±5%.
7. The surface cladding process for the inner hole of a large thin-walled cylindrical steering tube forging according to claim 1 is characterized by: When the substrate is 42CrMo, the powder composition for laser cladding in the laser cladding system equipment is Fe78.85%, C0.15%, Cr18.0%, Ni2.5%, Mo0.5% in weight percentage, and the total amount error is ±5%.