Wear-resistant protective coating for rapid repair of mining equipment and preparation method of wear-resistant protective coating
By applying high-hardness MCrAlY coating on mining equipment, the problems of insufficient hardness and low wear resistance after wear are solved, and high hardness and wear resistance in a wide temperature range are achieved, and low cost and environmental protection are achieved.
Patent Information
- Application Number
- CN202411144532.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the use of mining equipment, there are problems such as insufficient hardness, low wear resistance and short-term wear loss due to harsh environment and improper material selection.
Using a high-hardness MCrAlY coating, the NiCo alloy powder is dominated by adding elements such as Cr, Al2O3, Y, and supplemented with inorganic compounds such as Ti, B, Si, Cr3C2, SiC, CeO2, and dispersed through magnetic stirring, ultrasonic cleaning and ball mill. A 4.0-5.0mm thick wear-resistant protective coating is formed on the surface of the mining equipment using supersonic cold spraying process.
It achieves high hardness and excellent wear resistance in the range of room temperature to 1500°C, reduces costs, is environmentally friendly, and the interface between the coating and the substrate is balanced and coordinated, which significantly improves the wear resistance of the equipment.
Smart Images

Figure CN119020783A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wear-resistant protective coatings, in particular to a wear-resistant protective coating for rapid repair of mining equipment and a preparation method thereof. Background Art
[0002] Mining equipment refers to the mining, screening, transportation and other special equipment used in the mining production process, mainly refers to the mining, screening, transportation and other special equipment used in the production process of various mines such as coal, ferrous metals and non-ferrous metals. Mining equipment is prone to wear during use. The serious wear of mining equipment is mainly caused by factors such as its harsh working environment, harsh operating conditions and improper material selection, mainly including abrasive wear, adhesive wear and cavitation.
[0003] Mining equipment needs to be repaired after it is worn. The common mining equipment repair adopts welding technology. However, after welding, cracks still exist inside the equipment. The hardness of the welded position is generally not high, and the wear resistance is insufficient. It is still the original hardness of the substrate. In rare cases, a wear-resistant layer is applied to the repaired position. The common wear-resistant coating has low hardness and low temperature resistance, and there is a problem of coating wear in a short time. For this reason, we provide wear-resistant protective coatings for rapid repair of mining equipment and preparation methods thereof. Summary of the invention
[0004] The purpose of the present invention is to provide a wear-resistant protective coating for rapid repair of mining equipment and a preparation method thereof in view of the above technical problems. The wear-resistant protective coating for rapid repair of mining equipment and a preparation method thereof involved in the present invention are environmentally friendly, use less raw materials and have low cost; the high-hardness MCrAlY generated on the surface of the mining equipment repair position is uniform and dense, and has high hardness and excellent wear resistance within the service temperature range of room temperature to 1500°C.
[0005] To achieve this object, the present invention discloses a wear-resistant protective coating for rapid repair of mining equipment and a preparation method thereof, wherein the high-hardness MCrAlY coating is mainly composed of NiCo alloy powder: M represents NiCo, Cr represents metal Cr, AI represents Al2O3, and Y represents rare earth element Y, wherein the mass fraction of NiCo element is 45-52Wt.%, the mass fraction of Cr element is 19-27Wt.%, the mass fraction of Al2O3 element is 27-35Wt.%, and the mass fraction of Y element is 2-6Wt.%; the total mass fraction of auxiliary added elements or inorganic compounds is 6-10Wt.%.
[0006] In the above technical solution, the three main elements NiCo, Cr, Al2O3 and Y must be added simultaneously in the high hardness MCrAlY coating.
[0007] In the above technical solution, the high-hardness MCrAlY coating powder is mixed evenly by magnetic stirring, and the magnetic stirring parameters are: temperature 50-70° C., rotation speed 700-1000 r / min, and time 2-3 hours.
[0008] In the above technical solution, the auxiliary additive elements in the above high hardness MCrAlY coating include Ti, B, Si, Cr3C2, SiC, TiC, CeO2 or inorganic compounds, one or more of which are added.
[0009] In the above technical solution, the mixed coating powder in the high-hardness MCrAlY coating is cleaned with ultrasonic anhydrous ethanol and dried.
[0010] In the above technical solution, after the mixed powder of the high-hardness MCrAlY coating is dried, it is dispersed and ball-milled in a ball mill to obtain a particle size of 100 to 200 meshes.
[0011] The preparation method of the wear-resistant protective coating for rapid repair of mining equipment includes the following specific steps:
[0012] Step 1: sandblast and polish the position of the mining equipment to be repaired to obtain the mining equipment base;
[0013] Step 2: The mining equipment substrate obtained in step 1 is cleaned with ethanol;
[0014] Step 3: The mining equipment substrate with a clean surface obtained in step 2 is subjected to a spraying treatment by a supersonic cold spraying process, wherein the high-hardness MCrAlY powder is sprayed onto the surface of the mining equipment substrate by the supersonic cold spraying process to obtain a mining equipment having a high-hardness MCrAlY layer on the surface;
[0015] Step 4: Use the high-hardness MCrAlY coating powder and the process parameters of step 3 to prepare a wear-resistant protective coating on the substrate of the mining equipment with a thickness of 4.0 to 5.0 mm.
[0016] In the above technical solution, in step 1, the sandblasting parameters are spraying voltage 40V, spraying current 500A, powder feeding rate 45g·min-1, and spraying distance 80mm.
[0017] In the above technical solution, in step 3, the supersonic cold spraying process uses high-pressure helium or nitrogen as a carrier.
[0018] In the above technical solution, in step 3, the supersonic cold spraying process parameters are nitrogen pressure of 4-5MPa, spraying distance of 15-25mm, spray gun moving speed of 25-35mm / s, overlap of adjacent passes of 2-4mm, and spraying temperature of 800-1100°C.
[0019] The present invention has at least the following beneficial effects:
[0020] The high-hardness MCrAlY coating of the present invention is green and environmentally friendly, has low cost, and the NiCo-based coating obtained by the method of the present invention has a uniform surface and a balanced and coordinated interface between the coating and the substrate;
[0021] Auxiliary added elements or inorganic compounds such as Ti, B, Si, Cr3C2, SiC, TiC, CeO2, etc. can form precipitation or new compounds to fill the gaps between the coatings, thereby improving the density of the coatings;
[0022] The high-hardness MCrAlY coating of the present invention adds Ai2O3, and a part of the amorphous phase exists during the spraying process. During the spraying process, its cooling rate reaches the amorphous formation cooling rate, thereby forming an amorphous structure, and the mining equipment substrate and even the coating are further protected;
[0023] The generated high-hardness MCrAlY coating exhibits excellent high hardness and wear resistance in a wide temperature range from room temperature to 1500°C.
[0024] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A graph showing the relationship between the hardness and the test temperature of the substrate at the repair location of mining equipment and the coating prepared by Scheme 1 of the present invention;
[0026] Figure 2 A relationship diagram between the wear volume and the test temperature of the substrate at the repair position of mining equipment and the coating prepared by Scheme 1 of the present invention;
[0027] Figure 3 A graph showing the relationship between the hardness and the test temperature of the substrate at the repair location of mining equipment and the coating prepared by Scheme 2 of the present invention;
[0028] Figure 4 A relationship diagram between the wear volume and the test temperature of the substrate at the repair position of mining equipment and the coating prepared by Scheme 2 of the present invention;
[0029] Figure 5 The figure is a relationship diagram between the hardness and the test temperature of the existing cerakote coating and the coating prepared by scheme 3 of the present invention;
[0030] Figure 6 The figure is a relationship diagram between the wear volume and the test temperature of the existing cerakote coating and the coating prepared by scheme 3 of the present invention;
[0031] Figure 7It is a relationship diagram between the hardness and the test temperature of the existing nycote coating and the coating prepared by scheme 4 of the present invention;
[0032] Figure 8 It is a relationship diagram between the wear volume and the test temperature of the existing nycote coating and the coating prepared by scheme 4 of the present invention;
[0033] Fig. 9 SEM morphology of MCrAlY powder in high hardness MCrAlY coating;
[0034] Fig.10 SEM morphology of Al2O3 element in high hardness MCrAlY coating. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0036] The application principle of the present invention is described in detail below in conjunction with the accompanying drawings.
[0037] The high hardness MCrAlY coating is mainly composed of NiCo alloy powder: M represents NiCo, Cr represents metal Cr, AI represents Al2O3, and Y represents rare earth element Y, wherein the mass fraction of NiCo element is 40-48Wt.%, the mass fraction of Cr element is 19-27Wt.%, the mass fraction of Al2O3 element is 27-35Wt.%, and the mass fraction of Y element is 2-6Wt.%; the total mass fraction of auxiliary added elements or inorganic compounds is 2-7Wt.%.
[0038] Among them, the three main elements NiCo, Cr, Al2O3 and Y must be added simultaneously in the high hardness MCrAlY coating.
[0039] The high-hardness MCrAlY coating powder is evenly mixed by magnetic stirring, and the magnetic stirring parameters are: temperature 50-70° C., rotation speed 700-1000 r / min, and time 2-3 hours.
[0040] Among them, the auxiliary additive elements in the above-mentioned high hardness MCrAlY coating include Ti, B, Si, Cr3C2, SiC, TiC, CeO2 or inorganic compounds, one or more of which are added.
[0041] The mixed coating powder in the high-hardness MCrAlY coating is cleaned with ultrasonic anhydrous ethanol and dried.
[0042] The mixed powder of the high-hardness MCrAlY coating is dried and then dispersed and ball-milled with a ball mill to obtain a particle size of 100 to 200 meshes.
[0043] The preparation method of the wear-resistant protective coating for rapid repair of mining equipment includes the following specific steps:
[0044] Step 1: sandblast and polish the position of the mining equipment to be repaired to obtain the mining equipment base;
[0045] Step 2: The mining equipment substrate obtained in step 1 is cleaned with ethanol;
[0046] Step 3: The mining equipment substrate with a clean surface obtained in step 2 is subjected to a spraying treatment by a supersonic cold spraying process, wherein the high-hardness MCrAlY powder is sprayed onto the surface of the mining equipment substrate by the supersonic cold spraying process to obtain a mining equipment having a high-hardness MCrAlY layer on the surface;
[0047] Step 4: Use the high-hardness MCrAlY coating powder and the process parameters of step 3 to prepare a wear-resistant protective coating on the mining equipment substrate with a thickness of 4.0 to 5.0 mm.
[0048] Among them, in step 1, the sandblasting parameters are spraying voltage 40V, spraying current 500A, powder feeding rate 45g·min-1, and spraying distance 80mm.
[0049] Among them, in step 3, the supersonic cold spraying process uses high-pressure helium or nitrogen as a carrier.
[0050] Among them, in step 3, the supersonic cold spraying process parameters are nitrogen pressure of 4-5MPa, spraying distance of 15-25mm, spray gun moving speed of 25-35mm / s, overlap of adjacent passes of 2-4mm, and spraying temperature of 800-1100℃
[0051] Embodiment 1:
[0052] (1) Grinding treatment of the repair position of mining equipment: spraying voltage 40V, spraying current 500A, powder feeding rate 45g·min-1, spraying distance 80mm, and the obtained mining equipment substrate is then cleaned with ethanol to ensure the surface of the substrate is clean;
[0053] (2) Coating powder processing and mass fraction: In the high hardness MCrAlY powder, the mass fraction of NiCo element is 42wt.%, the mass fraction of Cr element is 20wt.%, the mass fraction of Al2O3 element is 30wt.%, and the mass fraction of Y element is 2wt.%. The mass fraction of auxiliary added Si element is 2wt.%, and the mass fractions of SiC and CeO2 are 2wt.% and 2wt.% respectively.
[0054] (3) The mixed coating powder is cleaned and dried by ultrasonic anhydrous ethanol, and the mixed powder is dispersed and milled by a ball mill after drying, and the particle size is 150-250 mesh.
[0055] (4) The process parameters of supersonic cold spraying are as follows: nitrogen pressure of 4-5 MPa, spraying distance of 15-25 mm, spray gun moving speed of 25-35 mm / s, overlap of adjacent passes of 2-4 mm, and spraying temperature of 800-1100 °C.
[0056] (5) The thickness of the wide temperature range wear-resistant protective coating prepared on the surface of the mining equipment repair location is 5.0 mm.
[0057] The experimental results show that:
[0058] After machining and polishing, the coating prepared in Scheme 1 has a uniform macroscopic surface and a dense structure. The coating in Scheme 1 maintains a high hardness in a wide temperature range from room temperature to 1500°C. The relationship between the hardness and temperature of the substrate and coating at the specific mining equipment repair location is as follows: Figure 1 The wear resistance of the coating in Scheme 1 has also been greatly improved, which is nearly 5 times higher than that of the substrate at the repaired position of the mining equipment. The relationship between the wear volume and temperature is shown in Figure 2 shown.
[0059] The hardness test found that the surface coating of the mine equipment repair location treated by the present invention had significantly increased hardness and reduced porosity compared with the substrate of the mine equipment repair location, indicating that the wear resistance of the coating of Scheme 1 was significantly improved, see Table 1.
[0060] Table 1 Analysis data of relevant parameters of substrate hardness of mining equipment repair location and coating in Scheme 2
[0061]
[0062] Embodiment 2:
[0063] (1) Grinding treatment of the repair position of mining equipment: spraying voltage 40V, spraying current 500A, powder feeding rate 45g·min-1, spraying distance 80mm, and the obtained mining equipment repair position substrate is then cleaned with ethanol to ensure the surface of the substrate is clean;
[0064] (2) Coating powder processing and mass fraction: In the high hardness MCrAlY powder, the mass fraction of NiCo element is 45Wt.%, the mass fraction of Cr element is 25Wt.%, the mass fraction of Al2O3 element is 19Wt.%, the mass fraction of Y element is 5Wt.%, the mass fraction of auxiliary added Si element is 2Wt.%, and the mass fractions of SiC and CeO2 are 2Wt.% and 2Wt.% respectively.
[0065] (3) The mixed coating powder is cleaned and dried by ultrasonic wave, and after drying, the mixed powder is dispersed and ball-milled by ball mill, and the particle size is 150-250 mesh.
[0066] (4) The process parameters of supersonic cold spraying are as follows: nitrogen pressure of 4-5 MPa, spraying distance of 15-25 mm, spray gun moving speed of 25-35 mm / s, overlap of adjacent passes of 2-4 mm, and spraying temperature of 800-1100 °C.
[0067] (5) The thickness of the wide temperature range wear-resistant protective coating prepared on the surface of the mining equipment repair location is 5.0 mm.
[0068] The experimental results show that:
[0069] After machining and polishing, the coating prepared in Scheme 2 has a uniform macroscopic surface and a dense structure. The coating in Scheme 2 maintains a high hardness in a wide temperature range from room temperature to 1500°C. The specific substrate at the repair location of the mining equipment and the relationship between the hardness and temperature of the coating in Scheme 2 are as follows: Figure 3 The wear resistance of the coating in Scheme 2 has also been improved, which is nearly 2 times higher than that of the substrate at the repaired position of the mining equipment. The relationship between the wear volume and temperature is shown in Figure 4 shown.
[0070] The hardness test found that the surface coating of the mine equipment repair location treated by the present invention had significantly increased hardness and reduced porosity compared with the substrate of the mine equipment repair location, indicating that the wear resistance of the coating of Scheme 2 was significantly improved, see Table 2.
[0071] Table 2 Analysis data of relevant parameters of substrate hardness of mining equipment repair location and coating in Scheme 1
[0072]
[0073]
[0074] Embodiment 3:
[0075] (1) Grinding treatment of the repair position of mining equipment: spraying voltage 40V, spraying current 500A, powder feeding rate 45g·min-1, spraying distance 80mm, and the obtained mining equipment substrate is then cleaned with ethanol to ensure the surface of the substrate is clean;
[0076] (2) Coating powder processing and mass fraction: In the high hardness MCrAlY powder, the mass fraction of NiCo element is 45wt.%, the mass fraction of Cr element is 19wt.%, the mass fraction of Al2O3 element is 28wt.%, the mass fraction of Y element is 2wt.%, the mass fraction of auxiliary added Si element is 2wt.%, and the mass fractions of SiC and CeO2 are 2wt.% and 2wt.% respectively.
[0077] (3) The mixed coating powder is cleaned and dried by ultrasonic anhydrous ethanol, and the mixed powder is dispersed and ball-milled by a ball mill after drying, and the particle size is 150-250 mesh.
[0078] (4) The process parameters of supersonic cold spraying are as follows: nitrogen pressure of 4-5 MPa, spraying distance of 15-25 mm, spray gun moving speed of 25-35 mm / s, overlap of adjacent passes of 2-4 mm, and spraying temperature of 800-1100 °C.
[0079] (5) The thickness of the wide temperature range wear-resistant protective coating prepared on the surface of the mining equipment repair location is 5.0 mm.
[0080] The experimental results show that:
[0081] After machining and polishing, the coating prepared in Scheme 3 has a uniform macroscopic surface and a dense structure. The coating in Scheme 3 maintains a high hardness in a wide temperature range from room temperature to 1500°C. The cerakote coating in the prior art is sprayed at different positions of the same equipment for comparison. The comparative relationship between hardness and temperature is shown in the figure. Figure 5 The wear resistance of the coating in Scheme 3 has also been greatly improved, which is significantly higher than that of the cerakote coating. The relationship between the wear volume and temperature is shown in Figure 6 shown.
[0082] The hardness test found that the surface coating of the repaired position of the mining equipment treated by the present invention had significantly increased hardness and reduced porosity compared with the cerakote coating. Although there was little difference in high temperature resistance, it showed that the wear resistance and strength of the coating of Scheme 3 were significantly improved, see Table 3.
[0083] Table 3 Analysis data of relevant parameters of substrate and coating hardness of mining equipment repair location in Scheme 3
[0084]
[0085] Example 4
[0086] (1) Grinding treatment of the repair position of mining equipment: spraying voltage 40V, spraying current 500A, powder feeding rate 45g·min-1, spraying distance 80mm, and the obtained mining equipment repair position substrate is then cleaned with ethanol to ensure the surface of the substrate is clean;
[0087] (2) Coating powder processing and mass fraction: In the high hardness MCrAlY powder, the mass fraction of NiCo element is 46Wt.%, the mass fraction of Cr element is 19Wt.%, the mass fraction of Al2O3 element is 27Wt.%, the mass fraction of Y element is 2Wt.%, the mass fraction of auxiliary added Si element is 2Wt.%, and the mass fractions of SiC and CeO2 are 2Wt.% and 2Wt.% respectively.
[0088] (3) The mixed coating powder is cleaned and dried by ultrasonic wave, and after drying, the mixed powder is dispersed and ball-milled by ball mill, and the particle size is 150-250 mesh.
[0089] (4) The process parameters of supersonic cold spraying are as follows: nitrogen pressure of 4-5 MPa, spraying distance of 15-25 mm, spray gun moving speed of 25-35 mm / s, overlap of adjacent passes of 2-4 mm, and spraying temperature of 800-1100 °C.
[0090] (5) The thickness of the wide temperature range wear-resistant protective coating prepared on the surface of the mining equipment repair location is 5.0 mm.
[0091] The experimental results show that:
[0092] After machining and polishing, the coating prepared in Scheme 4 has a uniform macroscopic surface and a dense structure. The coating in Scheme 4 maintains a high hardness in a wide temperature range from room temperature to 1500°C. The nycote coating in the prior art is sprayed at different positions of the same equipment for comparison. The comparative relationship between hardness and temperature is shown in the figure. Figure 7 The wear resistance of Scheme 4 coating has also been improved by 2 times, which is significantly better than that of nycote coating. The relationship between wear volume and temperature is shown in Figure 8 shown.
[0093] The hardness test found that the surface coating at the repaired position of the mining equipment treated by the present invention had significantly increased hardness and reduced porosity compared with the nycote coating, indicating that the wear resistance and strength of the coating of Scheme 4 were significantly improved, see Table 3.
[0094] Table 4 Analysis data of relevant parameters of substrate hardness of mining equipment repair location and coating in Scheme 4
[0095]
[0096] The wear-resistant protective coating for rapid repair of mining equipment of the present invention and its preparation method, the prepared high-hardness MCrAlY coating is environmentally friendly and low-cost, and the prepared coating has excellent high hardness and wear resistance in a wide temperature range of room temperature to 1500°C. The above embodiments are only used to illustrate but not limit the technical solutions of the present invention. Relevant technicians in this field can make reasonable modifications or equivalent substitutions to the present invention, but any modifications and partial substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of the claims of the present invention.
[0097] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
Claims
1. Wear-resistant protective coating for rapid repair of mining equipment, characterized in that: The high hardness MCrAlY coating is mainly composed of NiCo alloy powder: M represents NiCo, Cr represents metal Cr, AI represents Al2O3, and Y represents rare earth element Y, wherein the mass fraction of NiCo element is 45-52Wt.%, the mass fraction of Cr element is 19-27Wt.%, the mass fraction of Al2O3 element is 27-35Wt.%, and the mass fraction of Y element is 2-6Wt.%; the total mass fraction of auxiliary added elements or inorganic compounds is 6-10Wt.%.
2. The wear-resistant protective coating for rapid repair of mining equipment according to claim 1 is characterized in that: The three main elements NiCo, Cr, Al2O3 and Y must be added simultaneously in the above-mentioned high-hardness MCrAlY coating.
3. The wear-resistant protective coating for rapid repair of mining equipment according to claim 1 is characterized in that: The high-hardness MCrAlY coating powder is mixed evenly by magnetic stirring, and the magnetic stirring parameters are: temperature 50-70° C., rotation speed 700-1000 r / min, and time 2-3 hours.
4. The wear-resistant protective coating for rapid repair of mining equipment according to claim 1, characterized in that: The auxiliary additive elements in the above-mentioned high-hardness MCrAlY coating include Ti, B, Si, Cr3C2, SiC, TiC, CeO2 or inorganic compounds, one or more of which are added.
5. The wear-resistant protective coating for rapid repair of mining equipment according to claim 1, characterized in that: The mixed coating powder in the high-hardness MCrAlY coating is cleaned with ultrasonic anhydrous ethanol and dried.
6. The wear-resistant protective coating for rapid repair of mining equipment according to claim 1, characterized in that: The mixed powder of the high-hardness MCrAlY coating is dried and then dispersed and ball-milled in a ball mill to obtain a particle size of 150 to 250 meshes.
7. A method for preparing a wear-resistant protective coating for rapid repair of mining equipment, characterized in that: The specific steps include: Step 1: sandblast and polish the position of the mining equipment to be repaired to obtain the mining equipment base; Step 2: The mining equipment substrate obtained in step 1 is cleaned with ethanol; Step 3: The mining equipment substrate with a clean surface obtained in step 2 is subjected to a spraying treatment by a supersonic cold spraying process, wherein the high-hardness MCrAlY powder is sprayed onto the surface of the mining equipment substrate by the supersonic cold spraying process to obtain a mining equipment having a high-hardness MCrAlY layer on the surface; Step 4: Prepare a wear-resistant protective coating on the substrate of mining equipment according to the mixed powder ratio of claim 1 and the process parameters of step 3, with a thickness of 4.0 to 5.0 mm.
8. The preparation method according to claim 7, characterized in that: In step 1, the sandblasting parameters are spraying voltage 40V, spraying current 500A, powder feeding rate 45g·min-1, and spraying distance 80mm.
9. The preparation method according to claim 7, characterized in that: In step 3, the supersonic cold spray process uses high-pressure helium or nitrogen as a carrier.
10. The preparation method according to claim 7, characterized in that: In step 3, the supersonic cold spraying process parameters are nitrogen pressure of 4-5 MPa, spraying distance of 15-25 mm, spray gun movement speed of 25-35 mm / s, overlap of adjacent passes of 2-4 mm, and spraying temperature of 800-1100°C.
Citation Information
Cited By
Wear-resistant protective coating for rapid repair of mining equipment and preparation method of wear-resistant protective coating
CN120830074A