PAN-Ir / CNTs catalytic material as well as preparation method and application thereof

By growing iridium nanoparticles in situ on carbon nanotubes and anchoring them with polyacrylonitrile, PAN-Ir/CNTs catalytic material is formed, and the problem of rapid inactivation of iridium-based catalysts under acidic conditions is solved, achieving high activity and low cost and catalytic properties with strong stability, suitable for anode oxygen evolution reaction.

CN119020810APending Publication Date: 2024-11-26HENAN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411134924.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing iridium-based catalysts have high cost, low activity and instability problems in the anode oxygen evolution reaction, which leads to their limitations in large-scale applications, especially under acidic conditions, the catalyst is rapidly deactivated and difficult to meet industrial needs.

Method used

Using PAN-Ir/CNTs catalytic material, by growing iridium nanoparticles in situ on carbon nanotubes and anchoring iridium particles with polyacrylonitrile (PAN), the metal-support interaction is enhanced to form uniform size distribution and high stability. catalyst.

Benefits of technology

Under acidic conditions, PAN-Ir/CNTs catalytic materials exhibit excellent electrocatalytic activity and stability, low overpotential, good electrocatalytic stability, high mass activity, and can operate for a long time under high current density to maintain catalytic performance. , significantly reduces the amount and cost of iridium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020810A_ABST
    Figure CN119020810A_ABST
Patent Text Reader

Abstract

The invention discloses a PAN-Ir / CNTs catalytic material and a preparation method and application thereof, and relates to the field of electro-catalytic materials.According to the catalytic material, a carbon nano tube serves as a matrix, a carbon-loaded selenium film with reducibility is prepared firstly, then sub-nanoscale iridium particles grow on the carbon nano tube in situ through a replacement reaction between an Ir IV precursor and a selenium deposition film, and the PAN-Ir / CNTs catalytic material is obtained. According to the present invention, the carbon nano-tube is used as the carrier, such that the high dispersibility and the uniform size distribution of the iridium particles on the carbon nano-tube carrier are completely ensured, and the PAN is used to anchor the iridium nano-particles so as to further enhance the metal-carrier interaction (MSI) and inhibit the migration and the aggregation of the iridium nano-particles so as to provide the excellent stability of the catalyst; under the acidic condition, the PAN-Ir / CNTs catalytic material not only has excellent electrocatalytic activity, but also shows excellent catalytic durability, and is an acidic OER electrocatalyst with great potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrocatalytic materials, in particular to a PAN-Ir / CNTs catalytic material and a preparation method and application thereof. Background Art

[0002] Hydrogen is considered to be a potential energy source to replace fossil fuels, solving energy demand and environmental problems. Among the many hydrogen production technologies, proton exchange membrane (PEM) electrolyzer water electrolysis has attracted more attention due to its high conversion efficiency, large output, high hydrogen purity, and few by-products. Iridium-based materials are considered to be the preferred electrocatalysts for oxygen evolution reaction (OER) in PEM water electrolyzers. However, the high cost and relatively low OER activity of iridium are not enough to meet industrial requirements, which greatly limits the large-scale application of iridium-based catalysts in the future. In the past few decades, people have been studying the development of low-cost, high-activity new anode catalysts. For example, small-sized iridium or iridium oxide nanoparticles are dispersed on a carrier with a high surface area to improve the utilization rate of iridium, thereby reducing the amount of iridium to reduce costs. This measure can indeed increase the proportion of iridium atoms exposed outside the particles and improve the activity of iridium-based catalysts. However, small-sized nanoparticles are more likely to agglomerate and grow during the catalytic process, and fall off from the carrier, resulting in a rapid decrease in the catalytic activity of the catalyst. In general, how to design iridium-based catalysts that are highly active, low-cost and stable is still a bottleneck that plagues their large-scale use in the anode oxygen evolution reaction (OER).

[0003] The anodic oxygen evolution reaction (OER) has a high overpotential, low pH, and high oxygen concentration. The catalyst deactivation is mainly due to the following two reasons: one is Oswald ripening. When the size, shape, and distribution of the synthesized iridium nanoparticles are uneven, the corresponding surface energy is different, which leads to different solubility in the solvent. During the long OER catalytic process, in order to promote the system to reach thermodynamic equilibrium, small-sized nanoparticles will gradually dissolve, and these solutes will diffuse to the surface of larger particles and deposit, causing the large particles to gradually grow. Oswald ripening will lead to a significant reduction in the active sites of the catalyst and accelerate the deactivation of the catalyst. The second is when the metal-support interaction (MSI) between the synthesized iridium nanoparticles and the support is not strong enough. During the long OER catalytic process, the iridium atoms that are closer will combine at a faster dispersion speed to form larger particles, reducing the specific surface area of ​​the catalyst and causing the catalyst to deactivate.

[0004] In order to minimize the problem of catalyst deactivation, the synthesized catalyst should first have uniform size and shape to eliminate the difference in chemical potential between different particles, thereby minimizing Oswaldization. Secondly, there should be a stronger metal-support support effect (MSI) between the catalyst and the carrier to alleviate the problem of binding and shedding between nanoparticles. At present, the size and distribution of iridium nanocrystals can be effectively controlled by directly growing iridium nanoparticles in situ on carbon carriers in a one-step method. However, due to the inertness of carbon, it is also difficult for synthesized iridium nanoparticles to establish a strong metal-support interaction (SMSI) with the carbon carrier. The latest research shows that by establishing polymer and metal oxide coatings on the catalyst surface, such as polypyrrole and polyaniline, the catalyst can be protected from electrochemical oxidation and corrosion, thereby improving the stability of the catalyst. However, these polymers will inevitably cover some active sites of the nanocrystals.

[0005] Therefore, how to design iridium-based catalysts that are simultaneously highly active, low-cost and stable remains a bottleneck that plagues their large-scale use in the anodic oxygen evolution reaction (OER). Summary of the invention

[0007] In order to address the deficiencies in the prior art, the present invention provides a PAN-Ir / CNTs catalytic material and a preparation method and application thereof. The catalytic material prepared by the method of the present invention not only has excellent electrocatalytic activity under acidic conditions, but also exhibits excellent catalytic durability, and is a highly potential acidic OER electrocatalyst.

[0008] In order to achieve the above object, the specific scheme adopted by the present invention is: A method for preparing a PAN-Ir / CNTs catalytic material mainly comprises the following steps: (1) Preparation of selenium balls Selenious acid and polyvinyl pyrrolidone are dissolved in high-purity water at a mass ratio of 0.645:1, and ultrasonic stirring is performed until they are completely dissolved. Then, hydrazine hydrate is added and magnetic stirring is performed to allow the mixture to fully react at room temperature. The obtained product is centrifuged and washed to obtain nano-scale selenium spheres; (2) Preparation of carbon-supported selenium film The selenium balls prepared in step (1) are added with water to prepare a first solution, the carbon nanotubes are added with water to prepare a second solution, the first solution is added to the second solution, ultrasonicated until fully mixed, and the obtained product is centrifuged, dried, and annealed to obtain a carbon-supported selenium film; (3) In situ growth of iridium nanoparticles on carbon nanotubes The carbon-supported selenium film obtained in step (2) is added with water to prepare a third solution, chloroiridic acid is added, and after being uniformly dispersed by ultrasonication, a hydrothermal reaction is performed, and the product after the hydrothermal reaction is centrifuged, washed, and dried to obtain an Ir / CNTs intermediate, wherein iridium nanoparticles are in situ grown on the carbon nanotubes of the Ir / CNTs intermediate; (4) Preparation of PAN-Ir / CNTs catalytic materials The Ir / CNTs intermediate obtained in step (3) and polyacrylonitrile are dissolved in N,N-dimethylformamide at a mass ratio of 1:1.75, and ultrasonically stirred until completely dispersed. The obtained product is centrifuged, dried, and annealed to obtain a PAN-Ir / CNTs catalytic material.

[0009] Furthermore, in step (2), the concentration of the first solution is 1 to 2 mg mL -1 , the concentration of the second solution is 1 mg mL -1 , the volume ratio of the first solution to the second solution is 1:3.

[0010] Furthermore, in step (2), the drying conditions are vacuum drying, the drying temperature is 60 to 80° C., and the drying time is 8 to 12 hours.

[0011] Furthermore, in step (2), the annealing conditions are: heating at 180-250° C. for 1-3 h under an inert atmosphere.

[0012] Furthermore, in step (3), the concentration of the third solution is 0.5 to 1 mg mL -1 The volume ratio of the third solution to chloroiridic acid is 200:1, the hydrothermal reaction temperature is 120-150°C, and the hydrothermal time is 2-4h.

[0013] Furthermore, in step (3) or step (4), the drying condition is vacuum drying, the drying temperature is 60 to 80° C., and the drying time is 10 to 15 hours.

[0014] Furthermore, in step (4), the annealing condition is inert protection, and the temperature is kept at 300-400° C. for 1-3 hours.

[0015] On the one hand, the present invention discloses a PAN-Ir / CNTs catalytic material prepared by the above method.

[0016] Furthermore, using carbon nanotubes as carriers, a carbon-supported selenium film with reducing properties was first prepared, and then Ir IV The replacement reaction between the precursor and the selenium deposited film in situ grows ellipsoidal subnanometer iridium particles on carbon nanotubes, and then the iridium particles are anchored with PAN to further strengthen the metal-support interaction to obtain PAN-Ir / CNTs catalytic material.

[0017] In another aspect, the present invention discloses the use of the above PAN-Ir / CNTs catalytic material as a catalyst for anode oxygen evolution reaction.

[0018] Beneficial effects:

[0019] (1) When preparing the catalytic material of the present invention, carbon nanotubes are used as the matrix to first prepare a carbon-supported selenium film with reducing properties, and then Ir Ⅳ The replacement reaction between the precursor and the selenium deposited film in situ grows sub-nanometer iridium particles on the carbon nanotubes, which fully ensures the high dispersion and uniform size distribution of the iridium particles on the carbon nanotube support. The electrocatalytic performance of the catalyst is then greatly improved by anchoring the iridium nanoparticles with polyacrylonitrile (PAN). This is because polyacrylonitrile is a good surface coating material with potential activity, and its structure can be well adjusted by controlling the heat treatment temperature. As the temperature increases, linear polyacrylonitrile can gradually unfold into a network structure, thereby further strengthening the metal-support interaction (MSI), inhibiting the migration and aggregation of iridium nanoparticles, and giving the catalyst excellent stability. In addition, the strong electronic interaction between pyridinic nitrogen and Ir accelerates the adsorption of Ir on *OOH intermediates, promotes the rapid OER reaction, and improves the electrocatalytic activity of the catalyst.

[0020] (2) The PAN-Ir / CNTs catalytic material provided by the present invention has been experimentally confirmed to have the following excellent OER electrocatalytic activity and stability under acidic conditions, and can be used as an acidic OER electrocatalyst: (I) Extremely low overpotential The LSV test under acidic conditions shows that commercial Ir / C has a -2 At a current density of 10 mA cm, the overpotential is 333 mV, while PAN-Ir / CNTs-400 only needs 209 mV to reach 10 mA cm -2 of current density. (II) Excellent electrocatalytic stability Chronopotentiometry (CP) tests under acidic conditions show that commercial Ir / C has a high conductivity at 10 mA cm -2 The PAN-Ir / CNTs-400 was completely inactivated at 10 mA cm -2 After running stably for 500 h, the overpotential only dropped by 60 mV. (III) Higher mass activity The electrocatalyst mass activity was calculated by LSV curve. The mass activity of PAN-Ir / CNTs-400 at 1.50 V vs. RHE was as high as 1385.7 A g Ir -1 , which is 40 times higher than commercial Ir / C at 1.50V vs.RHE (34.7A g Ir -1 ). (IV) Excellent structural stability After 500 hours of stabilization, the morphology and structure of PAN-Ir / CNTs-400 of the present invention remain intact. In summary, the carbon nanotube-supported iridium nanoparticles anchored by polyacrylonitrile (PAN) with uniform size distribution and strong metal-support effect provided by the present invention have excellent OER electrocatalytic activity and stability under acidic conditions and can be used as an acidic OER electrocatalyst.

[0021] (3) The preparation method of the PAN-Ir / CNTs catalytic material provided by the present invention uses carbon nanotubes, which are widely available, as carriers and is synthesized through a replacement reaction under hydrothermal conditions. It has a high conversion efficiency and uses polyacrylonitrile to anchor iridium nanoparticles, which significantly improves its electrocatalytic performance, greatly saves costs, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of the synthesis of the catalytic material in Example 1.

[0023] Figure 2 The XRD diagrams of the products obtained in Examples 1-4 and Comparative Examples 1-3 are shown.

[0024] Figure 3 This is the TEM image of the product obtained in Example 1.

[0025] Figure 4 The iridium grain size diagram of the products obtained in Comparative Example 2 and Example 1.

[0026] Figure 5 HRTEM and unit cell diagram of the product obtained in Example 1

[0027] Figure 6 The XPS full spectrum (6(a)), Ir 4f spectrum (6(b)), and N1s spectrum (6(c)) of the products obtained in Examples 1-4 and Comparative Example 2 are shown.

[0028] Figure 7 The following are Fourier transform infrared spectra of the products obtained in Examples 1-4.

[0029] Figure 8 The linear sweep voltammetry (LSV) curves of the products obtained in Examples 1-4 and Comparative Examples 2-3 in a 0.5 M H2SO4 solution environment are shown in Figure 1. All curves are compensated by 90% iR, and the scan rate is 10 mV s -1 ; (b) Catalyst Tafel slope plot corresponding to the LSV curve.

[0030] Fig. 9 The mass activities and TOF values ​​of the products obtained in Example 1 and Comparative Examples 2-3 at 1.50 V vs. RHE.

[0031] Fig.10 In order to determine the stability of the products obtained in Example 1 and Comparative Examples 2-3 by chronopotentiometry (CP), at a given 10 mA cm -2 Under the current density, observe the voltage change with time.

[0032] Fig.11 TEM images of the products obtained in Example 1 and Comparative Example 2 after CP testing.

[0033] Fig.12 This is a grain size diagram of the products obtained in Example 1 and Comparative Example 2 after CP testing.

[0034] Fig.13 The CV records of the products obtained in Examples 1-4 and Comparative Examples 2-3 at different scan rates within the range of 1.0 to 1.1 V are shown.

[0035] Fig.14 C of the products obtained in Examples 1-4 and Comparative Examples 2-3 dl picture.

[0036] Fig.15 TEM images of the products obtained in Examples 2-4.

[0037] Fig.16 The LSV curves of the products obtained in Examples 1-4 and Comparative Examples 2-3 after ECSA normalization.

[0038] Fig.17 The impedance diagrams of the products obtained in Example 1 and Comparative Examples 2-3 are shown. DETAILED DESCRIPTION

[0039] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0040] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, reagents and materials used in the present invention are commercially available. It should be noted that, in the absence of conflict, the features in the embodiments of the present invention and the embodiments can be combined with each other. In order to enable those skilled in the art to better understand the technical scheme of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings.

[0041] Example 1

[0042] A preparation method of PAN-Ir / CNTs electrocatalyst material, please refer to Figure 1 , mainly includes the following steps: (1) Preparation of selenium spheres: 0.774 g of selenious acid and 1.2 g of polyvinylpyrrolidone (PVP) were dissolved in high-purity water, and ultrasonically stirred for 10 min until completely dissolved. 2.2 mL of hydrazine hydrate was added and magnetically stirred for 3 h to allow for sufficient reaction. The product was centrifuged (8000 r / min, 8 min) and washed (washed three times with high-purity water) to obtain selenium spheres with a diameter of about 50 nm. (2) Preparation of carbon-supported selenium film (Se / CNTs): Se spheres were added with water to a concentration of 2 mg mL -1 The first solution was prepared by adding water to carbon nanotubes to a concentration of 1 mg mL -1 The second solution of 20 mL of the first solution and 60 mL of the second solution were mixed; the mixture was ultrasonicated in an ice-water bath for 3 h, the product was collected by centrifugation (10000 r / min, 10 min), dried in a vacuum drying oven (60° C.) for 12 h, and then heat-treated at 250° C. for 2 h under argon protection to obtain a carbon-supported selenium film (Se / CNTs); (3) In situ growth of iridium particles on carbon nanotubes: 10 mg of Se / CNTs obtained in step (2) was diluted with water to obtain a concentration of 0.5 mg mL -1 The third solution, 100 μL of 500 mM chloroiridic acid was added to 20 mL of the third solution and stirred for 10 min. The above solution was poured into a 50 mL reactor, hydrothermally reacted at 150 ° C for 4 h, and after natural cooling, the obtained product was centrifuged at 20000 rpm for 10 min and washed three times with high-purity water. The product obtained by centrifugation was vacuum dried at 60 ° C for 12 h to obtain the final product Ir / CNTs intermediate; (4) Synthesis of PAN-Ir / CNTs nanocrystals: 20 mg Ir / CNTs and 35 mg PAN were dissolved in 20 mL N,N-dimethylformamide (DMF) solution. The solid was dissolved by ultrasound, and then reacted at 300 rpm / min under a magnetic stirrer for 12 h, and then centrifuged at 20,000 rpm for 10 min. The product obtained by centrifugation was vacuum dried at 60 °C for 12 h, and then heat treated at 400 °C for 2 h under argon protection. The obtained sample was labeled PAN-Ir / CNTs-400.

[0043] When preparing the catalytic material, the present invention first loads selenium nanospheres on carbon nanotubes by ultrasound, and then heat treats them at 250° C. for 2 h under argon protection to melt the selenium nanospheres, and then diffuses and evenly distributes them on the entire surface of the carbon nanotubes. The obtained sample is marked as Se / CNTs. During the heat treatment process, part of Se evaporates, and the Se atoms deposited on the carbon nanotubes can be used as a reducing agent to in-situ grow sub-nanometer iridium particles on the carbon nanotubes. The principle is as shown in formula (1): The sample obtained at this time is Ir / CNTs. In order to further improve its electrocatalytic performance, the prepared Ir / CNTs catalyst and polyacrylonitrile (PAN) are mixed in N,N-dimethylformamide (DMF) solution and magnetically stirred for 12 hours to allow polyacrylonitrile to fully contact with the catalyst. The obtained powder is treated at 400°C under argon protection for 1 hour to obtain the target product PAN-Ir / CNTs-400 after PAN anchoring.

[0044] Example 2

[0045] The difference between Example 2 and Example 1 is that in step (4), the heat treatment temperature is 300° C. and the obtained sample is labeled PAN-Ir / CNTs-300.

[0046] Example 3

[0047] The difference between Example 3 and Example 1 is that in step (4), the heat treatment temperature is 350° C. and the obtained sample is labeled PAN-Ir / CNTs-350.

[0048] Example 4

[0049] The difference between Example 4 and Example 1 is that in step (4), the heat treatment temperature is 450° C. and the obtained sample is labeled PAN-Ir / CNTs-450.

[0050] Comparative Example 1

[0051] The difference between Comparative Example 1 and Example 1 is that it does not include step (3) and step (4), and the obtained sample is a carbon-supported selenium film, denoted as Se / CNTs.

[0052] Comparative Example 2

[0053] The difference between Comparative Example 2 and Example 1 is that step (4) is not included, and the obtained sample is an Ir / CNTs intermediate, referred to as Ir / CNTs for short.

[0054] Comparative Example 3

[0055] The commercial Ir / C used in Comparative Example 3 was produced by MacLean.

[0056] The compositions of the products obtained in Examples 1-4 and Comparative Examples 1-3 were qualitatively analyzed by X-ray diffraction (XRD). Figure 2As shown, the diffraction peaks of Se and CNT can be clearly seen in Se / CNTs, while in Ir / CNTs, there is only the peak of CNTs and the diffraction peak of Se is not retained, which indicates that Se fully participates in the reaction as a reducing agent in this process. Since the iridium particles contained in the synthesized Ir / CNTs, PAN-Ir / CNTs-300, PAN-Ir / CNTs-350, PAN-Ir / CNTs-400 and PAN-Ir / CNTs-450 are sub-nanometer particles with a small content, the diffraction peak of iridium is not obviously detected. In order to further explore the morphology and structure of the material, the catalyst was characterized by TEM. Figure 3 The TEM image of PAN-Ir / CNTs-400 synthesized in this study is shown. The Ir nanoparticles show uniform size and distribution on the CNTs substrate. The size distribution analysis of 200 Ir particles shows that the particle size of Ir / CNTs is 1.13±0.27nm ( Figure 4 a), the size of Ir nanocrystals after heat treatment (1.28±0.19nm) is almost unchanged ( Figure 4 b). HRTEM analysis of PAN-Ir / CNTs-400 shows that the lattice fringe spacing is 0.221nm ( Figure 5 ), corresponding to the (111) plane of Ir (PDF No 87-0715). The periodic lattice runs through the entire nanoparticle, which also confirms the formation of a single crystal structure. It is well known that the atomic utilization is closely related to the size of the particle. For such an Ir cubic octahedron with a side length of only 1.28nm, its atomic utilization is very high, and the surface atomic ratio can reach 52%.

[0057] In order to better understand the chemical state of the synthesized catalyst, we further used X-ray photoelectron spectroscopy (XPS) to analyze the data. Figure 6 The signals of Ir 4f, N 1s, and C 1s can be clearly observed in a. Figure 6 b is the Ir 4f spectra of PAN-Ir / CNTs (Examples 1-4) and Ir / CNTs (Comparative Example 2) after heat treatment at different temperatures. The fitting peaks at 61.1 and 64.2 eV are zero-valent iridium (Ir 0 ), the peaks at 62.1 and 65.1 eV are oxidized iridium (Ir IV ), it can be clearly seen that zero-valent Ir is dominant in the prepared catalyst, and a small part exists in an oxidized state. According to different peak areas, compared with PAN-Ir / CNTs-300, the Ir of PAN-Ir / CNTs-400 is IVThe content of Ir increased from 14% to 28%, which indicates that with the increase of heat treatment temperature, Ir binds more strongly to the ligand (N) with stronger electron-attracting ability, resulting in tighter binding of the electrons outside the nucleus and gradually turning to the oxidized state (Ir IV ) transition. The three fitting peaks in the XPS spectrum of N 1s are 400.3, 399.6 and 398.6 eV ( Figure 6 c), which can be attributed to pyrrolic nitrogen, Ir-N bond and pyridinic nitrogen respectively. Compared with PAN-Ir / CNTs-300, the Ir-N content in PAN-Ir / CNTs-400 increased from 14% to 22%, which is consistent with the above Ir IV The results of the increase in the content of , indicating that there is an obvious electronic interaction between nitrogen atoms and iridium atoms, and it gradually increases with the increase of the content of Ir-N. In addition, the pyridinic nitrogen decreased from 57% of PAN-Ir / CNTs-300 to 51% of PAN-Ir / CNTs-350 and 45% of PAN-Ir / CNTs-400, and finally to 41% of PAN-Ir / CNTs-450. The reduction and change of N are consistent with previous studies, that is, during the heat treatment, the linear PAN changes from a step-type rich in pyridinic nitrogen to a defective network structure with a reduced number. According to the XPS results, the changes in the fitting peaks of nitrogen and iridium indicate that the introduction of pyridinic nitrogen causes a significant change in the electronic structure of the iridium surface, and any change in the electronic structure may affect the adsorption of intermediates, regulate the intrinsic pathways in the catalytic process, and affect the electrocatalytic activity and stability of the material.

[0058] The results of Fourier transform infrared spectroscopy (FTIR) further confirmed the above trend ( Figure 7 ). When the heat treatment temperature increases from 300℃ to 350℃, the -1 The nitrile group (C≡N) at 1610 cm -1 The C=N bond strength and vibration frequency decreased, and a "red shift" phenomenon occurred, indicating that PAN began to cyclize and initially formed nitrogen heterocycles (pyridine rings and pyrrole rings); when the temperature continued to rise from 350°C to 450°C, the C=N bond absorption peak continued to decrease, but the C≡N bond strength showed a slight increase trend. This may be due to further cross-linking reactions between PAN molecular chains, resulting in further destruction of C=N, the reformation of some C≡N bonds, and the gradual transformation of the carbon chain structure into a more stable and rigid ring structure, providing further evidence for improving the stability of the catalyst. According to XPS and Fourier transform infrared spectroscopy (FTIR) data, the structure of PAN can be well adjusted by controlling the heat treatment temperature to ensure that OER can be carried out efficiently and stably.

[0059] We evaluated the OER catalytic activity of the products obtained in Examples 1-4 and Comparative Examples 2-3 in an oxygen-saturated 0.5MH2SO4 solution using a three-electrode system. The instruments used for the test were Shanghai Chenhua CHI 760E. The electrodes were calibrated before the OER test. The glassy carbon electrode was used as the working electrode with a geometric area of ​​0.071 cm 2 , the mercurous sulfate electrode was used as the reference electrode, the platinum sheet was used as the counter electrode, and the polarization curve was normalized to the surface area of ​​the electrode.

[0060] When preparing the working electrode, 5 mg of the catalytic material was dispersed in 1 mL of a mixed solvent of water and isopropanol (1:3, v:v), and then 50 μL of Nafion (5 wt%) solution was added. The mixture was ultrasonicated for 40 min in an ice-water bath to form a well-dispersed ink. The ink was then dropped onto a pre-polished and cleaned glassy carbon electrode (GCE, diameter = 3 mm) and dried at room temperature to obtain a working electrode for electrochemical testing. The final Ir loading on the electrode was 0.281 mg cm -2 .

[0061] In the electrochemical test, the cyclic voltammogram (CV) was obtained in a room temperature N2-saturated H2SO4 solution with a scan rate of 5 mV s -1 , potential range 0.3-1.2 V vs. RHE, in the potential range 0.3-1.0 V vs. RHE, scan rate 5 mVs at room temperature -1 The OER activity was measured and 90% compensation was performed. The cyclic voltammetry curves of the electrochemical active area were 2-12 mV s -1 The EIS was measured at different scan rates with a frequency range of 100 kHz to 0.01 Hz, a potential of 1.3 V, and an amplitude potential of 5 mV. The current density of the catalyst test in the chronopotentiometry was 10 mA cm -2 .

[0062] like Figure 8 As shown in (a), at a current density of 10 mA cm -2 When , the overpotential of PAN-Ir / CNTs-400 is the lowest, which is 209mV, much lower than PAN-Ir / CNTs-450 (266mV), PAN-Ir / CNTs-350 (270mV), PAN-Ir / CNTs-300 (282mV), Ir / CNTs (302mV) and commercial Ir / C (333mV), indicating that the prepared PAN-Ir / CNTs-400 catalyst has the best electrocatalytic activity. The Tafel slope is obtained by fitting the polarization curve, as shown in Figure 8 (b) The Tafel slope of PAN-Ir / CNTs-400 is only 49.2 mV dec. -1, much smaller than PAN-Ir / CNTs-450 (63.1mV dec -1 ), PAN-Ir / CNTs-350 (63.2mV dec -1 ), PAN-Ir / CNTs-300 (97.3mV dec -1 )、Ir / CNTs(95.6mV dec -1 ) and commercial Ir / C (119.9mV dec -1 ), indicating that it has faster OER reaction kinetics, which is conducive to the rapid progress of OER reaction. In order to further explore the intrinsic activity of PAN-Ir / CNTs-400 catalyst, several catalyst mass activities were calculated at 1.50V vs.RHE, such as Fig. 9 As shown, PAN-Ir / CNTs-400 is as high as 1385.7Ag Ir -1 , which is 40 times higher than commercial Ir / C at 1.50V vs.RHE (34.7Ag Ir -1 ). This further confirmed that PAN-Ir / CNTs-400 is a very promising OER catalyst. PAN-Ir / CNTs-400 not only has excellent catalytic activity, but also exhibits excellent catalytic stability. Fig.10 As shown in the figure, the stability of PAN-Ir / CNTs-400 was tested by chronopotentiometry. -2 After continuous operation for 500 hours at a current density of 1.5 Å, the electrocatalytic performance only decayed by 60 mV, while the commercial Ir / C was completely deactivated after running for less than 50 hours. After long-term stability testing, the iridium nanoparticles in the Ir / CNTs that were not anchored by PAN all fell off, and the catalyst was completely ineffective ( Fig.11 (b)), while the structure of PAN-Ir / CNTs-400 is still very stable ( Fig.11 (a)), the iridium nanoparticles did not grow significantly ( Fig.12 ). In summary, PAN-Ir / CNTs-400 not only has excellent electrocatalytic activity, but also has excellent OER catalytic stability, and is a very promising oxygen evolution reaction electrocatalyst.

[0063] At 1, 2, 4, 6, 8, 10, 12 mV s -1 CV cycle scanning was carried out on different catalysts at a scanning rate of Fig.13 ), the double layer capacitance (C dl ) to evaluate the electrochemically active surface area (ESCA) ( Fig.14). Compared with Ir / CNTs and commercial Ir / C, the C of the PAN-modified catalyst increases with the increase of heat treatment temperature. dl Gradually decrease, specifically Com Ir / C (16mF cm -2 )<PAN-Ir / CNTs-450(27mF cm -2 )<PAN-Ir / CNTs-400(32mF cm -2 )<PAN-Ir / CNTs-350(44mF cm -2 )<PAN-Ir / CNTs-300(51mF cm -2 )<Ir / CNTs(55mF cm -2 ), which indicates that PAN successfully covers the catalyst surface, and the number of iridium active sites covered gradually increases with the increase of heat treatment temperature. Fig.15 The TEM results show that PAN-Ir / CNTs-300( Fig.15 (a))、PAN-Ir / CNTs-350( Fig.15 (b)), and the above-mentioned PAN-Ir / CNTs-400 catalyst ( Figure 3 ) surface did not aggregate, therefore, the reduction in ECSA can be largely attributed to the structural changes of PAN, which in turn adjusted the number of covered active sites, giving the catalyst excellent electrocatalytic performance, while PAN-Ir / CNTs-450( Fig.15 (c) The iridium nanoparticles at the edge of the catalyst agglomerated, resulting in a decrease in ECSA. It is worth noting that the electrocatalytic activity of most catalysts was not affected after PAN modification, such as Fig.16 is the LSV normalized by ECSA. With the increase of heat treatment temperature, the performance of the catalyst modified by PAN did not continue to improve. The electrocatalytic activity of PAN-Ir / CNTs-400 was significantly higher than that of Ir / CNTs and commercial Ir / C, while the electrocatalytic activity of PAN-Ir / CNTs-450 was lower than that of PAN-Ir / CNTs-400. This is consistent with the results of ECSA and TEM obtained above, that is, at the annealing temperature of 450°C, the catalyst itself agglomerated, resulting in a decrease in activity.

[0064] Electrochemical impedance spectroscopy is also often used to explore the reaction mechanism of catalysts. EIS tests were performed at open circuit voltage, such as Fig.17As shown in the figure, compared with the other two catalysts, PAN-Ir / CNTs-400 has a smaller internal resistance, indicating faster reaction kinetics, stronger adsorption capacity for the OER intermediate OOH*, and faster deprotonation rate in the OER reaction. This also further illustrates that the PAN-Ir / CNTs-400 we prepared is a very promising oxygen evolution reaction electrocatalyst.

[0065] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Any equivalent changes or modifications made according to the essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a PAN-Ir / CNTs catalytic material, characterized in that: The main steps are as follows: (1) Preparation of selenium balls Selenious acid and polyvinyl pyrrolidone are dissolved in high-purity water at a mass ratio of 0.645:1, and ultrasonically stirred until completely dissolved, and then hydrazine hydrate is added and magnetically stirred to fully react at room temperature. The obtained product is centrifuged and washed to obtain nano-scale selenium spheres; (2) Preparation of carbon-supported selenium thin film The selenium balls prepared in step (1) are added with water to prepare a first solution, the carbon nanotubes are added with water to prepare a second solution, the first solution is added to the second solution, ultrasonicated until fully mixed, and the obtained product is centrifuged, dried, and annealed to obtain a carbon-supported selenium film; (3) In situ growth of iridium nanoparticles on carbon nanotubes The carbon-supported selenium film obtained in step (2) is added with water to prepare a third solution, chloroiridic acid is added, and after ultrasonic dispersion, a hydrothermal reaction is performed. The product after the hydrothermal reaction is centrifuged, washed, and dried to obtain an Ir / CNTs intermediate, wherein iridium nanoparticles are in situ grown on the carbon nanotubes of the Ir / CNTs intermediate; (4) Preparation of PAN-Ir / CNTs catalytic materials The Ir / CNTs intermediate obtained in step (3) and polyacrylonitrile are dissolved in N,N-dimethylformamide at a mass ratio of 1:1.75, and ultrasonically stirred until completely dispersed. The obtained product is centrifuged, dried, and annealed to obtain a PAN-Ir / CNTs catalytic material.

2. The method for preparing a PAN-Ir / CNTs catalytic material according to claim 1, characterized in that: In step (2), the concentration of the first solution is 1-2 mg mL -1 , the concentration of the second solution is 1 mg mL -1 , the volume ratio of the first solution to the second solution is 1:

3.

3. The method for preparing a PAN-Ir / CNTs catalytic material according to claim 1, characterized in that: In step (2), the drying conditions are vacuum drying, the drying temperature is 60-80°C, and the drying time is 8-12 h.

4. The method for preparing a PAN-Ir / CNTs catalytic material according to claim 1, characterized in that: In step (2), the annealing conditions are: heating at 180-250 °C for 1-3 h under an inert atmosphere.

5. The method for preparing a PAN-Ir / CNTs catalytic material according to claim 1, characterized in that: In step (3), the concentration of the third solution is 0.5~1 mg mL -1 The volume ratio of the third solution to chloroiridic acid is 200:1, the hydrothermal reaction temperature is 120~150 ℃, and the hydrothermal time is 2~4 h.

6. The method for preparing a PAN-Ir / CNTs catalytic material according to claim 1, characterized in that: In step (3) or step (4), the drying conditions are vacuum drying, the drying temperature is 60-80°C, and the drying time is 10-15 h.

7. The method for preparing a PAN-Ir / CNTs catalytic material according to claim 1, characterized in that: In step (4), the annealing condition is inert protection, and the temperature is kept at 300~400℃ for 1-3 hours.

8. A PAN-Ir / CNTs catalytic material, characterized in that: The method is prepared by the method described in any one of claims 1 to 7.

9. The PAN-Ir / CNTs catalytic material according to claim 1, characterized in that: Using carbon nanotubes as carriers, a reductive carbon-supported selenium film was first prepared, and then Ir IV The replacement reaction between the precursor and the selenium deposited film in situ grows ellipsoidal subnanometer iridium particles on carbon nanotubes, and then the iridium particles are anchored with PAN to further strengthen the metal-support interaction to obtain PAN-Ir / CNTs catalytic material.

10. Use of the PAN-Ir / CNTs catalytic material according to any one of claims 8 to 9 as a catalyst for anode oxygen evolution reaction.