Preparation method of carrier-attached ultrathin copper foil and carrier-attached ultrathin copper foil

By forming a chromium carbon aluminum alloy peeling layer on the carrier copper foil and performing secondary electrodeposition of copper foil, the problem of unstable peeling strength between the carrier copper foil and ultra-thin copper foil is solved, and the stable and uniform peeling and applicability of the copper foil is achieved. promote.

CN119020836APending Publication Date: 2024-11-26SHANDONG JINBAO ELECTRONICS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411247554.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the peel strength between the carrier copper foil and the ultra-thin copper foil is unstable, resulting in too low or too high adhesive strength, affecting its usability, and making it difficult to peel evenly.

Method used

The chromium carbon aluminum alloy release layer is used to process the carrier copper foil through electrodeposition technology, and the copper foil is secondary electrodeposited at high temperature to form an ultra-thin copper foil with support to ensure the stability and uniformity of the release layer.

Benefits of technology

The delicate interface of the chromium carbon aluminum alloy layer is realized, the diffusion of copper foil is avoided, the stable and uniform peeling of ultra-thin copper foil is ensured, and its applicability is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005031255810000071
    Figure BDA0005031255810000071
  • Figure BDA0005031255810000081
    Figure BDA0005031255810000081
Patent Text Reader

Abstract

The invention relates to the technical field of electrolytic copper foil processing, in particular to a preparation method of carrier-attached ultrathin copper foil and the carrier-attached ultrathin copper foil. The invention provides a preparation method of a carrier-attached ultrathin copper foil. The preparation method comprises the following steps: (1) pretreating a carrier copper foil; (2) immersing the pretreated carrier copper foil into a stripping layer treatment solution, and carrying out primary electro-deposition to prepare a chromium-carbon-aluminum alloy stripping layer, so as to obtain a carrier copper foil with an alloy stripping layer; and (3) immersing the carrier copper foil with the alloy stripping layer into an electro-coppering solution, and carrying out secondary electro-deposition to obtain the carrier-attached ultrathin copper foil. According to the carrier-attached ultrathin copper foil prepared by the preparation method disclosed by the invention, the stripping force of the stripping layer is moderate, and the ultrathin copper foil can be easily, stably and uniformly separated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolytic copper foil processing, and in particular to a preparation method of an ultra-thin copper foil with a carrier and the ultra-thin copper foil with a carrier. Background Art

[0002] With the rapid development of technology in the world's electronic circuit industry, the chip-based and integrated applications of components are becoming more and more extensive. Electronic products will continue to develop in the direction of integration, automation, miniaturization, lightweight, and low energy consumption. In the future, the demand for high-end PCB products such as multilayer boards, rigid-flex boards, HDI boards, and IC substrates will increase significantly. The trend of downstream technology changes will promote the development of electronic circuit copper foil products and industrial technology upgrades.

[0003] The earliest major application field of ultra-thin copper foil with carrier is IC packaging substrate. Since 2017, the improved semi-additive method has been used to manufacture smartphone motherboards. Since the semi-additive process requires the use of ultra-thin copper foil with carrier, the demand for ultra-thin copper foil with carrier has increased. In actual production, the carrier foil needs to maintain a certain and uniform bonding force with the ultra-thin copper foil before pre-pressing, and after high-temperature pressing, the carrier foil should be easily peeled off from the solidified molded substrate material of the copper foil. It is pointed out in relevant research literature that the key problem in the production and use of carrier copper foil is to solve the peeling problem of the carrier foil and the ultra-thin copper foil, and ensure that there is appropriate peeling strength between them. When the peeling layer is uneven on the surface of the carrier foil, the bonding strength between the carrier foil and the ultra-thin copper foil will be unstable. Too low bonding strength will cause the two to separate prematurely and cannot be used; when the bonding strength is too strong, the ultra-thin copper foil is difficult to peel off from the carrier foil and cannot be used. Therefore, the peeling layer is a very important part of evaluating the applicability of the carrier copper foil, and its preparation is crucial. Summary of the invention

[0004] In order to solve the above technical problems existing in the prior art, the present invention provides a method for preparing an ultra-thin copper foil with a carrier and an ultra-thin copper foil with a carrier.

[0005] The technical solution of the present invention to solve the above technical problems is as follows:

[0006] A first aspect of the present invention is to provide a method for preparing an ultra-thin copper foil with a carrier, comprising the following steps:

[0007] (1) Pre-treating the carrier copper foil;

[0008] (2) immersing the pretreated carrier copper foil in a stripping layer treatment solution, and performing a first electrodeposition to prepare a chromium-carbon-aluminum alloy stripping layer, thereby obtaining a carrier copper foil with an alloy stripping layer;

[0009] (3) Immersing the carrier copper foil with the alloy release layer in a copper electroplating solution for secondary electrodeposition to obtain an ultra-thin copper foil with a carrier.

[0010] The beneficial effects of the present invention are as follows: the preparation method of the ultra-thin copper foil with a carrier provided by the present invention can produce an ultra-thin copper foil based on a chromium-carbon-aluminum alloy peeling layer, the chromium-carbon-aluminum alloy layer has fine grains and a pure interface, and can avoid diffusion between the copper foil and the peeling layer at high temperatures, so that the peeling force of the peeling layer is moderate, and the ultra-thin copper foil can be easily separated stably and evenly.

[0011] On the basis of the above technical solution, the present invention can also make the following technical improvements:

[0012] Furthermore, in step (1), the pretreatment is to immerse the carrier copper foil in a mixed aqueous solution of sulfuric acid and hydrogen peroxide for 15-60 seconds.

[0013] Furthermore, in the mixed aqueous solution of sulfuric acid and hydrogen peroxide, the volume ratio of sulfuric acid to water is 10-15%, and the volume ratio of hydrogen peroxide to water is 2%-5%.

[0014] The beneficial effect of adopting the above further technical solution is that oxides and oil stains on the surface of the carrier copper foil are fully removed, which is convenient for the subsequent electrodeposition process.

[0015] Furthermore, in step (2), the stripping layer treatment solution includes the following components in mass concentrations: 0.3-0.6 mol / L of chromium ion hexahydrate, 0.19-0.31 mol / L of oxalic acid dihydrate, 0.11-0.2 mol / L of tartaric acid, 0.11-0.2 mol / L of aluminum sulfate, and 0.1-0.2 mol / L of succinic acid.

[0016] Furthermore, in step (2), the peeling layer treatment solution uses pure water as a solvent, and the pH of the peeling layer treatment solution is 1-2.

[0017] Further, in step (2), the temperature of the primary electrodeposition is 30-40°C, and the current density is 20-25A / dm 2 The electrodeposition time is 5-10 seconds.

[0018] The beneficial effect of adopting the above further technical solution is that in step (2), the carrier foil is used as an electroplating cathode and placed in a stripping layer treatment solution for electroplating to obtain a stripping layer.

[0019] Furthermore, in step (3), the copper electroplating solution comprises the following components in mass concentrations: copper ion 70-100 g / L, sulfuric acid 90-110 g / L, chloride 5-10 ppm, and gelatin 2-10 ppm.

[0020] Further, in step (3), the current density of the secondary electrodeposition is 35-50A / dm 2, temperature is 40-60℃, time is 100-150 seconds.

[0021] Furthermore, the molecular weight of the gelatin is 50,000-100,000.

[0022] The beneficial effect of adopting the above further technical solution is that: in step (3), the carrier foil with the release layer in step (2) is used as an electroplating cathode and immersed in an electroplating copper solution to electrodeposit an ultra-thin copper foil.

[0023] Another aspect of the present invention is to provide an ultra-thin copper foil with a carrier, which is prepared by the above-mentioned preparation method.

[0024] Compared with the prior art, the present invention has the following technical effects:

[0025] By adopting the preparation method of the ultra-thin copper foil with a carrier provided by the present invention, the alloy peeling layer can be obtained in one step, the preparation method is simple, and the obtained ultra-thin copper foil with a carrier can be stably and evenly peeled off after high-temperature pressing. DETAILED DESCRIPTION

[0026] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0027] In the following examples and comparative examples, the chloride is selected from sodium chloride, the hexahydrated chromium ion is selected from chromium trichloride hexahydrate, and the copper ion is selected from copper sulfate.

[0028] Example 1

[0029] (1) Pre-treating the carrier copper foil, wherein the pre-treatment solution is a mixed aqueous solution of sulfuric acid and hydrogen peroxide, wherein the volume ratios of sulfuric acid, hydrogen peroxide and water are 10% and 5% respectively, and the immersion time is 20 seconds;

[0030] (2) Immersing the pretreated carrier copper foil in a stripping layer treatment solution to perform electrodeposition to prepare a chromium-carbon-aluminum alloy stripping layer, thereby obtaining a carrier copper foil with an alloy stripping layer. The stripping layer treatment solution comprises: pure water as a solvent, a hexahydrate chromium ion mass concentration of 0.3 mol / L, an oxalic acid dihydrate mass concentration of 0.23 mol / L, a tartaric acid mass concentration of 0.2 mol / L, an aluminum sulfate mass concentration of 0.2 mol / L, a succinic acid mass concentration of 0.15 mol / L, a pH of 1.1, a temperature of 30° C., and electrodeposition conditions as follows: a current density of 20 A / dm 2 , the deposition time is 10s;

[0031] (3) Immersing the carrier copper foil with the alloy peeling layer in an electroplating copper solution to perform electroplating of the ultra-thin copper foil to obtain an ultra-thin copper foil with a carrier, wherein the electroplating copper solution comprises: pure water as a solvent, a copper ion concentration of 70 g / L, a sulfuric acid concentration of 100 g / L, a chloride concentration of 5 ppm, a gelatin concentration of 5 ppm, a temperature of 45° C., and the electroplating conditions are as follows: a current density of 35 A / dm 2 , time 150s;

[0032] Among them, the molecular weight of gelatin is 80,000.

[0033] After testing, the peeling force results of the peeling layer are shown in Table 1.

[0034] Example 2

[0035] (1) Pre-treating the carrier copper foil, wherein the pre-treatment solution is a mixed aqueous solution of sulfuric acid and hydrogen peroxide, wherein the volume ratios of sulfuric acid, hydrogen peroxide and water are 15% and 3% respectively, and the immersion time is 60 seconds;

[0036] (2) Immersing the pretreated carrier copper foil in a stripping layer treatment solution to perform electrodeposition to prepare a chromium-carbon-aluminum alloy stripping layer, thereby obtaining a carrier with an alloy stripping layer. The stripping layer treatment solution comprises: pure water as a solvent, a hexahydrate chromium ion mass concentration of 0.4 mol / L, an oxalic acid dihydrate mass concentration of 0.29 mol / L, a tartaric acid mass concentration of 0.15 mol / L, an aluminum sulfate mass concentration of 0.12 mol / L, a succinic acid mass concentration of 0.2 mol / L, a pH of 1.5, a temperature of 35° C., and electrodeposition conditions as follows: a current density of 25 A / dm 2 , the deposition time is 5s;

[0037] (3) Immersing the carrier copper foil with the alloy peeling layer in an electroplating copper solution to prepare an ultra-thin copper foil by electroplating, thereby obtaining an ultra-thin copper foil with a carrier. The electroplating copper solution comprises: pure water as a solvent, a copper ion concentration of 80 g / L, a sulfuric acid concentration of 110 g / L, a chloride concentration of 9 ppm, a gelatin concentration of 2 ppm, a temperature of 50° C., and the electroplating conditions are as follows: a current density of 42 A / dm 2 , time 130s;

[0038] Among them, the molecular weight of gelatin is 100,000.

[0039] After testing, the peeling force results of the peeling layer are shown in Table 1.

[0040] Example 3

[0041] (1) Pre-treating the carrier copper foil, wherein the pre-treatment solution is a mixed aqueous solution of sulfuric acid and hydrogen peroxide, wherein the volume ratios of sulfuric acid, hydrogen peroxide and water are 13% and 4% respectively, and the immersion time is 40 seconds;

[0042] (2) The pretreated carrier copper foil is immersed in a stripping layer treatment solution to perform electrodeposition to prepare a chromium-carbon-aluminum alloy stripping layer, thereby obtaining a carrier with an alloy stripping layer. The stripping layer treatment solution comprises: pure water as a solvent, a hexahydrate chromium ion mass concentration of 0.6 mol / L, an oxalic acid dihydrate mass concentration of 0.2 mol / L, a tartaric acid mass concentration of 0.12 mol / L, an aluminum sulfate mass concentration of 0.15 mol / L, a succinic acid mass concentration of 0.18 mol / L, a pH of 2, a temperature of 40°C, and electrodeposition conditions as follows: a current density of 23 A / dm 2 , the deposition time is 8s;

[0043] (3) Immersing the carrier copper foil with the alloy peeling layer in an electroplating copper solution to perform electroplating of the ultra-thin copper foil to obtain an ultra-thin copper foil with a carrier, wherein the electroplating copper solution comprises pure water as a solvent, a copper ion concentration of 100 g / L, a sulfuric acid concentration of 100 g / L, a chloride concentration of 7 ppm, a gelatin concentration of 8 ppm, a temperature of 60° C., and the electroplating conditions are as follows: a current density of 50 A / dm 2 , time 100s;

[0044] Among them, the molecular weight of gelatin is 60,000.

[0045] After testing, the peeling force results of the peeling layer are shown in Table 1.

[0046] Comparative Example 1

[0047] (1) Pre-treating the carrier copper foil, wherein the pre-treatment solution is a mixed aqueous solution of sulfuric acid and hydrogen peroxide, wherein the volume ratios of sulfuric acid, hydrogen peroxide and water are 12% and 5%, respectively, and the immersion time is 20 seconds;

[0048] (2) The pretreated carrier copper foil was immersed in a stripping layer treatment solution. The stripping layer treatment solution composition was: pure water as solvent, oxalic acid dihydrate mass concentration of 0.2 mol / L, tartaric acid mass concentration of 0.12 mol / L, aluminum sulfate mass concentration of 0.15 mol / L, succinic acid mass concentration of 0.18 mol / L, pH of 2, temperature of 40°C, and electrodeposition conditions were as follows: current density of 23 A / dm 2 , the deposition time is 8s;

[0049] (3) The carrier copper foil with the peeling layer is immersed in the electroplating copper solution as the electroplating cathode to prepare the ultra-thin copper foil by electroplating, and the ultra-thin copper foil with the carrier is obtained. The electroplating copper solution is composed of pure water as the solvent, the copper ion concentration is 100 g / L, the sulfuric acid concentration is 100 g / L, the chloride concentration is 7 ppm, the gelatin concentration is 8 ppm, the temperature is 60°C, and the electroplating conditions are as follows: the current density is 50 A / dm 2 , time 100s;

[0050] Among them, the molecular weight of gelatin is 60,000.

[0051] After testing, the peeling force results of the peeling layer are shown in Table 1.

[0052] Comparative Example 2

[0053] (1) Pre-treating the carrier copper foil, wherein the pre-treatment solution is a mixed aqueous solution of sulfuric acid and hydrogen peroxide, wherein the volume ratios of sulfuric acid, hydrogen peroxide and water are 12% and 5% respectively, and the immersion time is 20 seconds;

[0054] (2) The pretreated carrier copper foil was immersed in a stripping layer treatment solution. The stripping layer treatment solution composition was: pure water as solvent, hexahydrate chromium ion mass concentration of 0.4 mol / L, tartaric acid mass concentration of 0.15 mol / L, succinic acid mass concentration of 0.2 mol / L, pH of 1.5, temperature of 35°C, and electrodeposition conditions were as follows: current density of 25 A / dm 2 , the deposition time is 5s;

[0055] (3) The carrier copper foil with the peeling layer is immersed in the electroplating copper solution as the electroplating cathode to prepare the ultra-thin copper foil by electroplating, and the ultra-thin copper foil with the carrier is obtained. The electroplating copper solution is composed of pure water as the solvent, the copper ion concentration is 100 g / L, the sulfuric acid concentration is 100 g / L, the chloride concentration is 7 ppm, the gelatin concentration is 8 ppm, the temperature is 60°C, and the electroplating conditions are as follows: the current density is 50 A / dm 2 , time 100s;

[0056] Among them, the molecular weight of gelatin is 60,000.

[0057] After testing, the peeling force results of the peeling layer are shown in Table 1.

[0058] Comparative Example 3

[0059] (1) Pre-treating the carrier copper foil, wherein the pre-treatment solution is a mixed aqueous solution of sulfuric acid and hydrogen peroxide, wherein the volume ratios of sulfuric acid, hydrogen peroxide and water are 10% and 5% respectively, and the immersion time is 20 seconds;

[0060] (2) Immersing the pretreated carrier copper foil in a stripping layer treatment solution to perform electrodeposition to prepare a chromium-carbon-aluminum alloy stripping layer, thereby obtaining a carrier copper foil with an alloy stripping layer. The stripping layer treatment solution comprises: pure water as a solvent, a hexahydrate chromium ion mass concentration of 0.25 mol / L, an oxalic acid dihydrate mass concentration of 0.35 mol / L, a tartaric acid mass concentration of 0.09 mol / L, an aluminum sulfate mass concentration of 0.3 mol / L, a succinic acid mass concentration of 0.4 mol / L, a pH of 1.3, a temperature of 30° C., and electrodeposition conditions as follows: a current density of 20 A / dm 2 , the deposition time is 10s;

[0061] (3) Immersing the carrier copper foil with the alloy peeling layer in an electroplating copper solution to perform electroplating of the ultra-thin copper foil to obtain an ultra-thin copper foil with a carrier, wherein the electroplating copper solution comprises: pure water as a solvent, a copper ion concentration of 70 g / L, a sulfuric acid concentration of 100 g / L, a chloride concentration of 5 ppm, a gelatin concentration of 5 ppm, a temperature of 45° C., and the electroplating conditions are as follows: a current density of 35 A / dm 2 , time 150s;

[0062] Among them, the chloride can be sodium chloride, and the molecular weight of gelatin is 80,000.

[0063] After testing, the peeling force results of the peeling layer are shown in Table 1.

[0064] Comparative Example 4

[0065] (1) Pre-treating the carrier copper foil, wherein the pre-treatment solution is a mixed aqueous solution of sulfuric acid and hydrogen peroxide, wherein the volume ratios of sulfuric acid, hydrogen peroxide and water are 15% and 3% respectively, and the immersion time is 60 seconds;

[0066] (2) Immersing the pretreated carrier copper foil in a stripping layer treatment solution to perform electrodeposition to prepare a chromium-carbon-aluminum alloy stripping layer, thereby obtaining a carrier with an alloy stripping layer. The stripping layer treatment solution comprises: pure water as a solvent, a hexahydrate chromium ion mass concentration of 0.4 mol / L, an oxalic acid dihydrate mass concentration of 0.29 mol / L, a tartaric acid mass concentration of 0.15 mol / L, a succinic acid mass concentration of 0.2 mol / L, a pH of 1.5, a temperature of 35° C., and electrodeposition conditions as follows: a current density of 25 A / dm2 , the deposition time is 5s;

[0067] (3) Immersing the carrier copper foil with the alloy peeling layer in an electroplating copper solution to prepare an ultra-thin copper foil by electroplating, thereby obtaining an ultra-thin copper foil with a carrier. The electroplating copper solution comprises: pure water as a solvent, a copper ion concentration of 80 g / L, a sulfuric acid concentration of 110 g / L, a chloride concentration of 9 ppm, a gelatin concentration of 2 ppm, a temperature of 50° C., and the electroplating conditions are as follows: a current density of 42 A / dm 2 , time 130s;

[0068] Among them, the molecular weight of gelatin is 100,000.

[0069] After testing, the peeling force results of the peeling layer are shown in Table 1.

[0070] After the ultra-thin copper foil with carrier was prepared, the peeling force of the peeling layer was tested. The testing instrument was a SHIMADZU-EZ-LX tensile testing machine. The test results are shown in Table 1.

[0071] Table 1 Peeling force of the embodiments and comparative examples

[0072]

[0073]

[0074] Note: In Table 1, Max is the maximum peeling force, Min is the minimum peeling force, and Avg is the average value of all peeling force data within the test sampling range.

[0075] According to the data results in Table 1, it can be seen that the peeling forces of the peeling layers of Examples 1, 2, and 3 are uniform and moderate, while the peeling force data of Comparative Example 1 is relatively small, the peeling force data of Comparative Examples 2 and 4 are relatively large, and the peeling force value of Comparative Example 3 is slightly uneven.

[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an ultra-thin copper foil with a carrier, characterized in that: The following steps are involved: (1) Pre-treating the carrier copper foil; (2) immersing the pretreated carrier copper foil in a stripping layer treatment solution, and performing a first electrodeposition to prepare a chromium-carbon-aluminum alloy stripping layer, thereby obtaining a carrier copper foil with an alloy stripping layer; (3) Immersing the carrier copper foil with the alloy release layer in a copper electroplating solution for secondary electrodeposition to obtain an ultra-thin copper foil with a carrier.

2. The method for preparing the ultra-thin copper foil with a carrier according to claim 1, characterized in that: In step (1), the pretreatment is to immerse the carrier copper foil in a mixed aqueous solution of sulfuric acid and hydrogen peroxide for 15-60 seconds.

3. The method for preparing the ultra-thin copper foil with a carrier according to claim 2, characterized in that: In the mixed aqueous solution of sulfuric acid and hydrogen peroxide, the volume ratio of sulfuric acid to water is 10-15%, and the volume ratio of hydrogen peroxide to water is 2%-5%.

4. The method for preparing the ultra-thin copper foil with a carrier according to claim 1, characterized in that: In step (2), the stripping layer treatment solution includes the following components in mass concentrations: 0.3-0.6 mol / L of chromium ion hexahydrate, 0.19-0.31 mol / L of oxalic acid dihydrate, 0.11-0.2 mol / L of tartaric acid, 0.11-0.2 mol / L of aluminum sulfate, and 0.1-0.2 mol / L of succinic acid.

5. The method for preparing the ultra-thin copper foil with a carrier according to claim 1, characterized in that: In step (2), the stripping layer treatment solution uses pure water as a solvent, and the pH of the stripping layer treatment solution is 1-2.

6. The method for preparing the ultra-thin copper foil with a carrier according to claim 1, characterized in that: In step (2), the temperature of the primary electrodeposition is 30-40°C and the current density is 20-25A / dm 2 The electrodeposition time is 5-10 seconds.

7. The method for preparing the ultra-thin copper foil with a carrier according to claim 1, characterized in that: In step (3), the copper electroplating solution includes the following components in mass concentrations: copper ion 70-100 g / L, sulfuric acid 90-110 g / L, chloride 5-10 ppm, and gelatin 2-10 ppm.

8. The method for preparing the ultra-thin copper foil with a carrier according to claim 1, characterized in that: In step (3), the current density of the secondary electrodeposition is 35-50A / dm 2 , temperature is 40-60℃, time is 100-150 seconds.

9. The method for preparing the ultra-thin copper foil with a carrier according to claim 7, characterized in that: The molecular weight of the gelatin is 50,000-100,000.

10. An ultra-thin copper foil with a carrier, characterized in that: The method is prepared according to any one of claims 1 to 9.

Citation Information

Cited By

  • Carrier copper foil and preparation method and application thereof

    CN122039171A