Method for preparing Cr (23-x) FexC6 single crystal and prepared crystal material

Through the four-arc single crystal lifting furnace and vacuum arc smelting technology, high-quality large-block Cr(23-x)FexC6 single crystals were prepared, solving the problems of low growth efficiency and low reproducibility in traditional methods, achieving high Purity and large volume single crystal preparation.

CN119020848AActive Publication Date: 2024-11-26WUHAN UNIV OF SCI & TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410815689.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-26
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

The traditional single crystal growth method has low growth efficiency, complicated operations and difficult to ensure the growth conditions of gradient doped single crystals, low process reproduction rate, and it is difficult to prepare high-quality large-scale Cr(23-x)FexC6 single crystals.

Method used

Cr(23-x)FexC6 single crystal was prepared by a four-arc single crystal lifting furnace, and uniform alloy ingot was formed by a vacuum arc melting furnace, and the lifting method was prepared in a four-arc single crystal lifting furnace, and the arc needle was used to heat and Rotating lifting needles to grow single crystals, avoid oxidation risks, reduce internal stress, and improve purity.

Benefits of technology

The preparation of large high-quality Cr(23-x)FexC6 single crystals is achieved, which improves the purity and volume of the single crystals, reduces production time, avoids the appearance of impurities, and improves the repeatability of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020848A_ABST
    Figure CN119020848A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of crystal preparation, and particularly relates to a method for preparing Cr (23-x) FexC6 single crystals and a prepared crystal material. The preparation method comprises the following steps that (1) a mixed metal ingot of Cr, Fe and C is prepared, and the molar ratio of Cr to Fe to C is (23-x): x: 1; (2) putting the mixed metal ingot obtained in the step (1) into a four-arc single crystal pulling furnace; and (3) vacuumizing the four-arc single crystal pulling furnace to 10 <-4 > torr, protecting by using protective gas, and preparing the Cr (23-x) FexC6 single crystal by using a pulling method under the current of 13-15A. According to the method, the high-purity Cr (23-x) FexC6 single crystal is prepared by adopting the four-arc single crystal pulling furnace, and a large-block high-quality single crystal sample can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of crystal preparation, and specifically relates to a method for preparing Cr (23-x) Fe x C6 single crystal method and the crystal material prepared. Background Art

[0002] Magnetic field, like chemical composition, temperature and pressure, is an important factor affecting phase transition. It is generally believed that carbides exhibit paramagnetism under high temperature and strong magnetic field, and the magnetic field has no effect on them. Experimental results show that stable alloy carbides will precipitate prematurely under the action of strong magnetic field. This result completely challenges the traditional view. For example, heat-resistant steel was tempered in a constant strong magnetic field of 12 Tesla, and the precipitation of alloy carbide M7C3 induced by strong magnetic field was observed and analyzed by transmission electron microscopy (Materials&Design 221(2022)111023). Carbide M 23 C6 has a giant magnetic moment because the magnetic moment of Fe atoms is 27% higher than that of pure iron. 23 C6 will have a strong response to the magnetic field, which in turn affects the creep properties of heat-resistant steel under high temperature and strong magnetic fields. This response has two meanings: first, the 3d orbital electronic structure (including charge, spin and orbit) and lattice structure of Fe atoms in carbides and the rebalance of their interactions all produce microscopic responses to the external field; second, the carbide M 23 Response of C6 precipitation characteristics such as size, content, and distribution to strong magnetic field.

[0003] Traditional single crystal growth methods include solid phase reaction method, flux method, optical floating zone method, etc. Although the quality of single crystals can be improved by adjusting the ratio of reactants and the thermal sintering process, the use of traditional processes to achieve gradient doping of samples has the disadvantages of low growth efficiency and complicated operation. It is also difficult to ensure the growth conditions of each gradient single crystal, and the process reproducibility is low. Summary of the invention

[0004] In order to solve the shortcomings of the prior art, the present invention provides a method for preparing Cr (23-x) Fe x The present invention adopts a four-arc single crystal pulling furnace to prepare high-purity Cr (23-x) Fe x C6 single crystal, can obtain large pieces of high-quality single crystal samples.

[0005] The technical solution provided by the present invention is as follows:

[0006] A method for preparing Cr (23-x) Fe x C6 single crystal method, using four arc single crystal pulling furnace to prepare Cr (23-x)Fe x C6 single crystal, wherein x=0, 1, 2 or 3.

[0007] The present invention adopts a four-arc single crystal pulling furnace to produce large blocks of high-quality Cr (23-x) Fe x C6 single crystal sample.

[0008] Preparation of Cr (23-x) Fe x The method for C6 single crystal specifically comprises the following steps:

[0009] 1) preparing a mixed metal ingot of Cr, Fe and C, wherein the molar ratio of Cr, Fe and C is (23-x):x:1;

[0010] 2) placing the mixed metal ingot obtained in step 1) into a four-arc single crystal pulling furnace;

[0011] 3) Evacuate the four-arc single crystal pulling furnace to 10 -4 torr, then protected with protective gas, and then Cr was prepared by Czochralski method at a current of 13-15A. (23-x) Fe x C6 single crystal.

[0012] Based on the above technical solution, Cr, Fe and C can be used as raw materials to prepare Cr (23-x) Fe x C6 single crystal sample.

[0013] Preferably, the current in step 3) is 14A, or about 14A.

[0014] Specifically, the step 1) includes the following steps:

[0015] a) weighing Cr, Fe and C raw materials in a molar ratio of (23-x):x:1;

[0016] b) placing the raw material obtained in step a) into a vacuum arc melting furnace;

[0017] c) The vacuum arc melting furnace is evacuated and filled with protective gas, and then an electric current is applied to melt the raw materials into ingots, and finally cooled to room temperature.

[0018] Specifically, in step a): weigh out single substance raw materials of Cr, Fe and C in a glove box filled with argon.

[0019] Based on the above technical solution, the risk of raw material oxidation can be avoided.

[0020] Specifically, in step b), the single substance raw material weighed in step a) is taken out by isolating it from the air with tin foil, and is placed in a vacuum arc melting furnace.

[0021] Based on the above technical solution, the risk of raw material oxidation can be avoided.

[0022] Specifically, in step c): In step c): multiple melting of both the front and back sides is performed; annealing is performed by furnace cooling.

[0023] Based on the above technical solution, multiple melting on both sides of the ingot is performed in a vacuum arc melting furnace to ensure the uniformity of the ingot; after melting, an annealing treatment is required to reduce internal stress to prevent explosion during pulling.

[0024] Specifically, in step 3), the rising rate of the lifting needle is 3.5-4.5 mm / h, preferably 4 mm / h, or about 4 mm / h.

[0025] Based on the above technical solution, a crystalline material with large grains can be obtained.

[0026] The present invention also provides Cr prepared by the above method (23-x) Fe x C6 crystal material.

[0027] The prepared Cr (23-x) Fe x C6 can achieve crystal rods 6-8cm long.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The present invention uses high-purity iron powder, chromium powder and carbon powder in different proportions as single-element raw materials, fully sintering them in a vacuum arc melting furnace, and multiple and full fusion of the front and back sides of the alloy ingot to form a uniform alloy ingot. The alloy ingot formed by multiple arc melting has uniform composition and low internal stress, and is not easy to break when stimulated by instantaneous local high temperature. Before melting in the vacuum arc melting furnace and the four-arc single crystal melting furnace, the method of heating the metal ingot with an arc needle is used to eliminate oxygen that may exist in the device, further reduce impurities that may appear in the growing single crystal, and improve the purity of the target product.

[0030] The single crystals of each component product obtained by the present invention have higher quality and larger overall volume, and compared with the flux method, the time for producing single crystals is greatly reduced.

[0031] The Cr obtained by the present invention (23-x) Fe x C6 can be used as a magnetic research material. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is the XRD diagram of each embodiment.

[0033] Figure 2 The optical photographs of various embodiments are shown in FIG. DETAILED DESCRIPTION

[0034] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0035] Example 1

[0036] The single crystal Cr prepared in this embodiment 23 The C6 method is as follows:

[0037] In a glove box filled with argon protection, 8.4889 g of chromium particles and 0.5111 g of carbon blocks were weighed according to the molar ratio, wrapped tightly with tin foil, and after the gas inside was pressed out, they were moved out of the glove box to a vacuum arc melting furnace.

[0038] Preparation of Cr 23 C6 Alloy Ingot

[0039] After wiping the inner wall of the vacuum arc melting furnace with alcohol, pour in the weighed powder and adjust the position of the arc needle. After adjustment, evacuate the arc melting furnace, first using a mechanical pump and then a molecular pump, until the appropriate vacuum degree is reached (the reading is about 10 -3 pa) stop vacuuming, fill with argon until the pressure is slightly above 0, turn on the power to start the arc. Use the arc needle to aim at the center of the titanium ingot and melt for about 7 minutes to deoxidize; then move the arc needle to the sample to be melted for melting; for the first melting, melt around the sample for a week, and then focus on heating and melting the center. Be careful not to bring the arc needle too close to the sample to prevent the particle sample from being blown away; after uniform droplets are formed, turn the alloy ingot over to continue melting the second side, each side should be fully and evenly heated, and finally cool to room temperature with the furnace, and take out the single crystal ingot.

[0040] Preparation of Cr 23 C6 single crystal

[0041] Wipe the inner wall and sample stage of the four-arc single crystal pulling furnace with alcohol, grind the pulling needle to a suitable degree, install five tungsten needles (arc needles) and pulling needles used for melting; 23 Place the C6 alloy ingot on the sample stage of the four-arc single crystal pulling furnace, adjust the sample stage, arc needle and pulling needle to the appropriate position; evacuate to 10 -4torr, fill with argon until the pressure is slightly above 0, turn on the arc needle for melting the titanium ingot, and melt for about 7 minutes to deoxidize; then turn on the other four arc needles to heat and melt the four sides of the alloy ingot until the current is about 14A. At this time, the alloy ingot is in a liquid molten state. Slowly insert the pulling needle into the center of the alloy ingot, fine-tune the current to a stable state, set the pulling needle to move slowly upward, turn on the rotation of the sample stage and the pulling needle, and continuously adjust the angle of the arc needle during the pulling process so that the sample adheres to the solid single crystal on the pulling needle, and the entire alloy ingot is in a liquid molten state. The whole process needs to last for more than 5 hours until a crystal rod of about 6 cm is grown; break the crystal rod in a mortar to obtain a large piece of crystal. This crystal is like Figure 2 As shown in part (1).

[0042] Example 2

[0043] The single crystal Cr prepared in this embodiment 22 The method of FeC6 is as follows:

[0044] In a glove box filled with argon protection, 8.0312 g of chromium particles, 0.3930 g of iron particles and 0.5049 g of carbon blocks were weighed according to the molar ratio, wrapped tightly with tin foil, and after the gas inside was pressed out, they were moved out of the glove box to a vacuum arc melting furnace.

[0045] Preparation of Cr 22 FeC6 alloy ingot

[0046] After wiping the inner wall of the vacuum arc melting furnace with alcohol, pour in the weighed powder and adjust the position of the arc needle. After adjustment, evacuate the arc melting furnace, first using a mechanical pump and then a molecular pump, until the appropriate vacuum degree is reached (the reading is about 10 -3 pa) stop vacuuming, fill with argon until the pressure is slightly above 0, turn on the power to start the arc. Use the arc needle to aim at the center of the titanium ingot and melt for about 7 minutes to deoxidize; then move the arc needle to the sample to be melted for melting; for the first melting, melt around the sample for a week, and then focus on heating and melting the center. Be careful not to bring the arc needle too close to the sample to prevent the particle sample from being blown away; after uniform droplets are formed, turn the alloy ingot over to continue melting the second side, each side should be fully and evenly heated, and finally cool to room temperature with the furnace, and take out the single crystal ingot.

[0047] Preparation of Cr 22 FeC6 single crystal

[0048] Wipe the inner wall and sample stage of the four-arc single crystal pulling furnace with alcohol, grind the pulling needle to a suitable degree, install five tungsten needles (arc needles) and pulling needles used for melting; 22Place the FeC6 alloy ingot on the sample stage of the four-arc single crystal pulling furnace, adjust the sample stage, arc needle and pulling needle to the appropriate position; evacuate to 10 -4 torr, fill with argon until the pressure is slightly above 0, turn on the arc needle for melting the metal ingot, and melt for 7 minutes to deoxidize; then turn on the other four arc needles to heat and melt the four sides of the alloy ingot until the current is about 14A. At this time, the alloy ingot is in a liquid molten state. Slowly insert the pulling needle into the center of the alloy ingot, fine-tune the current to a stable state, set the pulling needle to move slowly upward, turn on the rotation of the sample stage and the pulling needle, and continuously adjust the angle of the arc needle during the pulling process so that the sample adheres to the solid single crystal on the pulling needle, and the entire alloy ingot is in a liquid molten state. The whole process needs to last for more than 5 hours until a crystal rod of about 7 cm is grown; break the crystal rod in a mortar to obtain a large piece of crystal. This crystal is like Figure 2 As shown in part (2).

[0049] Example 3

[0050] The single crystal Cr prepared in this embodiment 21 The method of Fe2C6 is as follows:

[0051] In a glove box filled with argon protection, 7.5651 g of chromium particles, 0.7748 g of iron particles and 0.4981 g of carbon blocks were weighed according to the molar ratio, wrapped tightly with tin foil, and after the gas inside was pressed out, they were moved out of the glove box to a vacuum arc melting furnace.

[0052] Preparation of Cr 21 Fe2C6 alloy ingot

[0053] After wiping the inner wall of the vacuum arc melting furnace with alcohol, pour in the weighed powder and adjust the position of the arc needle. After adjustment, evacuate the arc melting furnace, first using a mechanical pump and then a molecular pump, until the appropriate vacuum degree is reached (the reading is about 10 -3 pa) stop vacuuming, fill with argon until the pressure is slightly above 0, turn on the power to start the arc. Use the arc needle to aim at the center of the titanium ingot and melt for about 7 minutes to deoxidize; then move the arc needle to the sample to be melted for melting; for the first melting, melt around the sample for a week, and then focus on heating and melting the center. Be careful not to bring the arc needle too close to the sample to prevent the particle sample from being blown away; after uniform droplets are formed, turn the alloy ingot over to continue melting the second side, each side should be fully and evenly heated, and finally cool to room temperature with the furnace, and take out the single crystal ingot.

[0054] Preparation of Cr 21 Fe2C6 single crystal

[0055] Wipe the inner wall and sample stage of the four-arc single crystal pulling furnace with alcohol, grind the pulling needle to a suitable degree, install five tungsten needles (arc needles) and pulling needles used for melting; 21 Place the Fe2C6 alloy ingot on the sample stage of the four-arc single crystal pulling furnace, adjust the sample stage, arc needle and pulling needle to the appropriate position; evacuate to 10 -4 torr, fill with argon until the pressure is slightly above 0, turn on the arc needle for melting the titanium ingot, and melt for 7 minutes to deoxidize; then turn on the other four arc needles to heat and melt the four sides of the alloy ingot until the current is about 14A. At this time, the alloy ingot is in a liquid molten state. Slowly insert the pulling needle into the center of the alloy ingot, fine-tune the current to a stable state, set the pulling needle to move slowly upward, turn on the rotation of the sample stage and the pulling needle, and continuously adjust the angle of the arc needle during the pulling process so that the sample adheres to the solid single crystal on the pulling needle, and the entire alloy ingot is in a liquid molten state. The whole process needs to last for more than 5 hours until a crystal rod of about 6 cm is grown; break the crystal rod in a mortar to obtain a large piece of crystal. This crystal is like Figure 2 As shown in part (3).

[0056] Example 4

[0057] The single crystal Cr prepared in this embodiment 20 The method of Fe3C6 is as follows:

[0058] In a glove box filled with argon protection, 7.3531 g of chromium particles, 1.1866 g of iron particles and 0.5085 g of carbon blocks were weighed according to the molar ratio, wrapped tightly with tin foil, and after the gas inside was pressed out, they were moved out of the glove box to a vacuum arc melting furnace.

[0059] Preparation of Cr 20 Fe3C6 alloy ingot

[0060] After wiping the inner wall of the vacuum arc melting furnace with alcohol, pour in the weighed powder and adjust the position of the arc needle. After adjustment, evacuate the arc melting furnace, first using a mechanical pump and then a molecular pump, until the appropriate vacuum degree is reached (the reading is about 10 -3 pa later), stop vacuuming, fill with argon until the pressure is slightly above 0, turn on the power to start the arc. Use the arc needle to aim at the center of the titanium ingot and melt for 7 minutes to deoxidize; then move the arc needle to the sample to be melted for melting; for the first melting, melt around the sample for a week, and then focus on heating and melting the center. Be careful not to bring the arc needle too close to the sample to prevent the particle sample from being blown away; after uniform droplets are formed, turn the alloy ingot over to continue melting the second side, and each side should be fully and evenly heated, and finally cool to room temperature with the furnace, and take out the single crystal ingot.

[0061] Preparation of Cr 20 Fe3C6 single crystal

[0062] Wipe the inner wall and sample stage of the four-arc single crystal pulling furnace with alcohol, grind the pulling needle to a suitable degree, install five tungsten needles (arc needles) and pulling needles used for melting; 20 Place the Fe3C6 alloy ingot on the sample stage of the four-arc single crystal pulling furnace, adjust the sample stage, arc needle and pulling needle to the appropriate position; evacuate to 10 -4 torr, fill with argon until the pressure is slightly above 0, turn on the arc needle for melting the titanium ingot, and melt for about 7 minutes to deoxidize; then turn on the other four arc needles to heat and melt the four sides of the alloy ingot until the current is about 14A. At this time, the alloy ingot is in a liquid molten state. Slowly insert the pulling needle into the center of the alloy ingot, fine-tune the current to a stable state, set the pulling needle to move slowly upward, turn on the rotation of the sample stage and the pulling needle, and continuously adjust the angle of the arc needle during the pulling process so that the sample adheres to the solid single crystal on the pulling needle, and the entire alloy ingot is in a liquid molten state. The whole process needs to last for more than 5 hours until a crystal rod of about 6 cm is grown; break the crystal rod in a mortar to obtain a large piece of crystal. This crystal is like Figure 2 As shown in part (4).

[0063] Test Case

[0064] like Figure 1 Shown are XRD diagrams of the crystalline materials of Examples 1 to 4. It can be seen from the diagram that the spectra of the materials of each example have basically no impurity peaks and the purity is greater than 99%.

[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. Preparation of Cr (23-x) Fe x The method for C6 single crystal is characterized by: Preparation of Cr using a four-arc single crystal pulling furnace (23-x) Fe x C6 single crystal, wherein x=0, 1, 2 or 3.

2. Preparation of Cr according to claim 1 (23-x) Fe x The method for C6 single crystal is characterized in that, The following steps are involved: 1) preparing a mixed metal ingot of Cr, Fe and C, wherein the molar ratio of Cr, Fe and C is (23-x):x:1; 2) placing the mixed metal ingot obtained in step 1) into a four-arc single crystal pulling furnace; 3) Evacuate the four-arc single crystal pulling furnace to 10 -4 torr, then protected with protective gas, and then Cr was prepared by Czochralski method at a current of 13-15A. (23-x) Fe x C6 single crystal.

3. Preparation of Cr according to claim 2 (23-x) Fe x The method for C6 single crystal is characterized in that, The step 1) comprises the following steps: a) weighing Cr, Fe and C raw materials in a molar ratio of (23-x):x:1; b) placing the raw material obtained in step a) into a vacuum arc melting furnace; c) The vacuum arc melting furnace is evacuated and filled with protective gas, and then an electric current is applied to melt the raw materials into ingots, and finally cooled to room temperature.

4. The method for preparing Cr according to claim 3 (23-x) Fe x The method for C6 single crystal is characterized in that, In step a), single substance raw materials of Cr, Fe and C are weighed in a glove box filled with argon.

5. The method for preparing Cr according to claim 3 (23-x) Fe x The method for C6 single crystal is characterized in that, In step b), the single substance raw material weighed in step a) is taken out by isolating it from air with tin foil, and is placed in a vacuum arc melting furnace.

6. The method for preparing Cr according to claim 3 (23-x) Fe x The method for C6 single crystal is characterized in that, In step c), the front and back sides are melted multiple times; and annealing is performed by furnace cooling.

7. The method for preparing Cr according to any one of claims 1 to 6. (23-x) Fe x The method for C6 single crystal is characterized in that, In step 3), the lifting rate of the lifting needle is 3.5-4.5 mm / h.

8. A Cr prepared according to any one of claims 1 to 7 (23-x) Fe x C6 crystal material.

Citation Information

Patent Citations

  • Preparation method of iron, copper, manganese and nickle high-entropy alloy

    CN109576519A

  • Eutectic high-entropy alloy and preparation method thereof

    CN110499445A

  • Four-arc Czochralski growth method of CeRu2Si2 single crystal

    CN110644044A

  • Iron-based amorphous alloy powder, preparation method of iron-based amorphous alloy powder and application of iron-based amorphous alloy powder in laser cladding

    CN113174547A

  • Vacuum arc melting method and vacuum arc melting furnace

    JP2010261689A