Preparation method of bacteriostatic antistatic polylactic acid fiber

By introducing carbon nanotube grafted polyhexamethylbiguanide hydrochloride bonded glycidyl ether into polylactic acid fiber, the problem of insufficient antistatic and antibacterial properties of polylactic acid fiber is solved, and excellent mechanics are prepared Performance and long-acting antistatic and antibacterial fibers are suitable for medical surgical gowns and surgical bed covers, reducing charge accumulation and risk of bacterial infection.

CN119020882APending Publication Date: 2024-11-26FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411318959.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Polylactic fibers have poor antistatic and antibacterial properties in medical surgical gowns and surgical bedspreads, leading to charge accumulation and risk of bacterial infection, affecting the normal operation of the equipment and the safety of patients.

Method used

Carbon nanotube grafted polyhexamethylbiguanide hydrochloride bonded glycidyl ether as antibacterial antistatic agent, combining polylactic acid, polyadipate butylene terephthalate and diisoperoxide Bacteria-anti-anti-static polylactic fibers are prepared by melt blending, primary drafting and secondary drafting processes.

Benefits of technology

The prepared fiber has excellent long-term antistatic, antibacterial properties and mechanical properties, high tensile strength, stable resistivity, significant antibacterial effect on bacteria, and can be completely biodegradable. It is suitable for medical surgical gowns and surgical bed covers. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020882A_ABST
    Figure CN119020882A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an antibacterial antistatic polylactic acid fiber, and belongs to the technical field of chemical fiber preparation. The polylactic acid fiber is prepared by taking polylactic acid as a matrix, poly (butylene adipate-co-terephthalate) as a toughening agent, dicumyl peroxide as an initiator and carbon nanotube grafted polyhexamethyl biguanide hydrochloride bonded glycerol glycidyl ether as an antibacterial antistatic agent through melt blending, primary drafting and secondary drafting. The prepared polylactic acid fiber has excellent long-acting antistatic property, antibacterial property and mechanical property, can be completely biodegraded, is suitable for manufacturing medical surgical gown and surgical bedspread, and has remarkable economic value and social benefit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical fiber preparation, and specifically relates to a method for preparing antibacterial and antistatic polylactic acid fiber. Background Art

[0002] Polylactic acid fiber is a new type of fully biodegradable polymer material with good biocompatibility and high strength. It is often used in textile, packaging and biomedical fields. However, the low polarity of polylactic acid molecules leads to poor antistatic properties. Therefore, when polylactic acid fibers are used to make medical surgical gowns and surgical bed covers, they are prone to charge accumulation on their surfaces due to repeated friction during use. These charges will attract dust and discharge instantaneously. The instantaneous discharge current will seriously affect the normal operation of medical surgical electronic equipment. At the same time, the poor antibacterial properties of polylactic acid can easily cause patients to be infected with bacteria during surgery, which can lead to life-threatening risks for patients during surgery. Summary of the invention

[0003] In view of the problems that the current polylactic acid fiber has poor antistatic and antibacterial properties when used to make medical surgical gowns and surgical bed covers, the present invention provides a method for preparing antibacterial and antistatic polylactic acid fiber. The polylactic acid fiber has excellent long-term antistatic, antibacterial and mechanical properties, and is completely biodegradable. It is used to make medical surgical gowns and surgical bed covers, which has significant economic value and social benefits.

[0004] To achieve the above object, the present invention adopts the following technical solution: The invention discloses an antibacterial and antistatic polylactic acid fiber, which is prepared by melt blending, primary drawing and secondary drawing with polylactic acid as a matrix, polybutylene adipate terephthalate as a toughening agent, dicumyl peroxide as an initiator and carbon nanotube grafted polyhexamethylbiguanide hydrochloride bonded glycerol glycidyl ether as an antibacterial and antistatic agent.

[0005] The preparation method of the antibacterial and antistatic polylactic acid fiber specifically comprises the following steps: (1) First, 2-4 g of carbon nanotubes were added to 50-200 mL of 40% ethanol solution by weight, and ultrasonically dispersed at room temperature for 10-30 min. Then, 3-9 g of polydopamine and 0.02-0.1 g of tris(hydroxymethyl)aminomethane hydrochloride) were added, and magnetic stirring was performed at room temperature for 12-24 h. After separation, washing, drying and crushing, polydopamine-modified carbon nanotubes were obtained. (2) Under nitrogen atmosphere, first add 2-6 g of polyhexamethylbiguanidine hydrochloride into 40-100 mL of dimethyl sulfoxide, and ultrasonically disperse at room temperature for 10-30 min. Then add 2-4 g of polydopamine-modified carbon nanotubes, and magnetically stir at 40-60 °C for 10-30 min. Finally, add 3-12 g of glycerol glycidyl ether, and continue magnetically stirring at 60-80 °C for 4-6 h. After separation, washing, drying and pulverization, carbon nanotubes grafted with polyhexamethylbiguanidine hydrochloride bonded with glycerol glycidyl ether are obtained. (3) According to the proportion, polylactic acid, polybutylene adipate terephthalate, diisopropylbenzene peroxide and carbon nanotube grafted polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether are kneaded at 165-185° C. for 6-10 minutes, and the kneaded product is crushed, stretched once, and stretched twice to obtain the polylactic acid fiber.

[0006] Furthermore, the carbon nanotubes in step (1) have a length of 3-12 μm and a diameter of 8-15 nm.

[0007] Furthermore, in parts by weight, the amounts of the materials used in step (3) are: 20-40 parts of polylactic acid, 2-6 parts of polybutylene adipate terephthalate, 0.2-0.8 parts of diisopropylbenzene peroxide, and 0.5-2 parts of carbon nanotube-grafted polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether.

[0008] Furthermore, the process conditions for the primary stretching in step (3) are as follows: the temperatures of each section of the twin-screw extruder are 165°C, 175°C, 185°C and 175°C, the extrusion speed is 0.64 m / min, and the pulling speed is 3.2 m / min.

[0009] Furthermore, the process conditions of the secondary drawing in step (3) are: heating temperature of 70-90°C, drawing multiple of 4-6 times, and winding speed of 0.5-1 m / min.

[0010] The significant advantages of the present invention are: (1) Carbon nanotubes are conductive nanomaterials with excellent performance. In order to maintain the high conductivity and dispersibility of carbon nanotubes, the present invention modifies the surface of carbon nanotubes with polydopamine through the π-π interaction between polydopamine and carbon nanotubes, so as to give the surface of carbon nanotubes abundant amino groups or hydroxyl groups. At the same time, the present invention grafts polyhexamethylbiguanide hydrochloride, which is a broad-spectrum fungicide, onto carbon nanotubes through the hydrogen bonding between the hydroxyl and amino groups of polydopamine and the amino groups of polyhexamethylbiguanide hydrochloride, thereby achieving the purpose of uniformly dispersing polyhexamethylbiguanide hydrochloride.

[0011] (2) Glycerol glycidyl ether is a commonly used compatibilizer for polylactic acid and polybutylene adipate terephthalate composites. The present invention first chemically bonds glycerol glycidyl ether to carbon nanotube grafted polyhexamethylbiguanide hydrochloride through a ring-opening reaction between the amino group of polyhexamethyleneguanidine hydrochloride and the epoxy group of glycerol glycidyl ether, and then performs a ring-opening reaction between the terminal carboxyl group or terminal hydroxyl group of polylactic acid and polybutylene adipate terephthalate and the epoxy group of glycerol glycidyl ether bonded to carbon nanotube grafted polyhexamethylbiguanide hydrochloride under the action of diisopropylbenzene peroxide, so that the carbon nanotube grafted polyhexamethylbiguanide hydrochloride bonded glycerol glycidyl ether is uniformly and stably dispersed in the mixed material.

[0012] (3) Polybutylene adipate terephthalate can give polylactic acid fiber excellent toughness, and the uniformly and stably dispersed carbon nanotubes grafted polyhexamethyl biguanide hydrochloride bonded glycerol glycidyl ether can give polylactic acid fiber excellent long-term antistatic, antibacterial and mechanical properties. At the same time, polylactic acid, polybutylene adipate terephthalate, carbon nanotubes, polydopamine, polyhexamethyl biguanide hydrochloride and glycerol glycidyl ether are all harmless to the human body and biodegradable materials. Therefore, the polylactic acid fiber prepared by the present invention has excellent long-term antistatic, antibacterial and mechanical properties, and its tensile strength is 191~215 MPa, the elongation at break is 69.2~77.3%, and the resistivity before and after the durability test is 3.32×10 8 ~6.24×10 8 Ω·cm and 5.94×10 8 ~1.32×10 9 Ω·cm, the antibacterial rates against Escherichia coli are 86.16~91.75% and 83.38~90.67%, and the antibacterial rates against Staphylococcus aureus are 86.45~92.33% and 84.64~92.15%, respectively. It is completely biodegradable and suitable for making medical surgical gowns and surgical bed covers, with significant economic value and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is the infrared absorption spectrum of carbon nanotube grafted polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether prepared in Example 1. DETAILED DESCRIPTION

[0014] The specific steps of preparing an antibacterial and antistatic polylactic acid fiber are as follows: (1) First, 2-4 g of carbon nanotubes were added to 50-200 mL of 40% ethanol solution by weight, and ultrasonically dispersed at room temperature for 10-30 min. Then, 3-9 g of polydopamine and 0.02-0.1 g of tris(hydroxymethyl)aminomethane hydrochloride) were added, and magnetic stirring was performed at room temperature for 12-24 h. After separation, washing, drying and crushing, polydopamine-modified carbon nanotubes were obtained. (2) Under nitrogen atmosphere, first add 2-6 g of polyhexamethylbiguanidine hydrochloride into 40-100 mL of dimethyl sulfoxide, and ultrasonically disperse at room temperature for 10-30 min. Then add 2-4 g of polydopamine-modified carbon nanotubes, and magnetically stir at 40-60 °C for 10-30 min. Finally, add 3-12 g of glycerol glycidyl ether, and continue magnetically stirring at 60-80 °C for 4-6 h. After separation, washing, drying and pulverization, carbon nanotubes grafted with polyhexamethylbiguanidine hydrochloride bonded with glycerol glycidyl ether are obtained. (3) 20-40 g of polylactic acid, 2-6 g of polybutylene adipate terephthalate, 0.2-0.8 g of diisopropylbenzene peroxide and 0.5-2 g of carbon nanotube-grafted polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether are kneaded at 165-185 °C for 6-10 min, and the kneaded product is crushed, stretched once, and stretched twice to obtain the polylactic acid fiber.

[0015] The carbon nanotubes in step (1) have a length of 3-12 μm and a diameter of 8-15 nm.

[0016] The process conditions of the primary stretching in step (3) are: the temperatures of each section of the twin-screw extruder are 165°C, 175°C, 185°C and 175°C, the extrusion speed is 0.64 m / min, and the pulling speed is 3.2 m / min. The process conditions of the secondary stretching are: the heating temperature is 70-90°C, the stretching multiple is 4-6 times, and the winding speed is 0.5-1 m / min.

[0017] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0018] Example 1 (1) First, 3 g of carbon nanotubes (length 3-12 μm, diameter 8-15 nm) were added to 120 mL of 40% ethanol solution by weight, and ultrasonically dispersed at room temperature for 20 min. Then, 6 g of polydopamine and 0.06 g of tris(hydroxymethyl)aminomethane hydrochloride were added, and magnetic stirring was performed at room temperature for 18 h. After separation, washing, drying and crushing, polydopamine-modified carbon nanotubes were obtained. (2) Under nitrogen atmosphere, 4 g of polyhexamethylbiguanide hydrochloride was first added to 70 mL of dimethyl sulfoxide, and ultrasonically dispersed at room temperature for 20 min. Then, 3 g of polydopamine-modified carbon nanotubes was added, and magnetic stirring was continued at 50 °C for 20 min. Finally, 8 g of glycerol glycidyl ether was added, and magnetic stirring was continued at 70 °C for 5 h. After separation, washing, drying and pulverization, carbon nanotubes grafted with polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether were obtained. (3) 30 g of polylactic acid, 4 g of poly(butylene adipate terephthalate), 0.5 g of diisopropylbenzene peroxide and 1.2 g of carbon nanotube-grafted poly(hexamethylbiguanide hydrochloride) bonded with glycerol glycidyl ether were kneaded at 175 ℃ for 8 min. The kneaded product was crushed, stretched once and stretched twice to obtain antibacterial and antistatic polylactic acid fiber. During the first stretching, the temperatures of each section of the twin-screw extruder were 165 ℃, 175 ℃, 185 ℃ and 175 ℃, the extrusion speed was 0.64 m / min, and the pulling speed was 3.2 m / min. During the second stretching, the heating temperature was 80 ℃, the stretching ratio was 5 times, and the winding speed was 0.8 m / min.

[0019] Figure 1 The infrared absorption spectrum of the carbon nanotube grafted with polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether prepared in this example is shown in the figure. As can be seen from the figure, in the infrared absorption spectrum of the polydopamine-modified carbon nanotube, the wave number is 3500 cm -1 The absorption peaks on the left and right are the stretching vibration absorption peaks of hydroxyl groups, with wave numbers ranging from 3000 to 2800 cm -1 The absorption peak that appears is the CH stretching vibration absorption peak of methine, which indicates that polydopamine has been successfully modified on the surface of carbon nanotubes. By comparing the infrared absorption spectra of carbon nanotubes modified with polydopamine, polyhexamethylbiguanide hydrochloride, and glycerol glycidyl ether, it can be found that in the infrared absorption spectrum of carbon nanotubes grafted with polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether, at a wave number of 3500cm -1 The hydroxyl stretching vibration absorption peak of polydopamine appeared around 3300 cm -1 The amino stretching vibration absorption peak belonging to polyhexamethylbiguanide hydrochloride appeared around 3000~2800 cm -1 The methylene and methine CH stretching vibration absorption peaks belonging to polydopamine, polyhexamethylbiguanide hydrochloride, and glycerol glycidyl ether appeared at a wave number of 1638 cm -1 The characteristic absorption peak of guanidine belonging to polyhexamethylbiguanide hydrochloride appeared at a wave number of 1235 cm -1 and 749 cm -1 The characteristic absorption peak of the epoxy group of glycerol glycidyl ether appeared at a wave number of 1010 cm−1 New characteristic absorption peaks attributed to the reaction of epoxy groups with amino groups to form C-OH appeared at , which indicated that carbon nanotubes grafted with polyhexamethylbiguanidine hydrochloride bonded with glycerol glycidyl ether were successfully prepared.

[0020] Example 2 (1) First, 2 g of carbon nanotubes (length 3-12 μm, diameter 8-15 nm) were added to 50 mL of 40% by weight ethanol solution, and ultrasonically dispersed at room temperature for 10 min. Then, 3 g of polydopamine and 0.02 g of tris(hydroxymethyl)aminomethane hydrochloride were added, and magnetic stirring was performed at room temperature for 12 h. After separation, washing, drying, and crushing, polydopamine-modified carbon nanotubes were obtained. (2) Under nitrogen atmosphere, 2 g of polyhexamethylbiguanide hydrochloride was first added to 40 mL of dimethyl sulfoxide, and ultrasonically dispersed at room temperature for 10 min. Then, 2 g of polydopamine-modified carbon nanotubes was added, and magnetic stirring was continued at 40 °C for 30 min. Finally, 3 g of glycerol glycidyl ether was added, and magnetic stirring was continued at 60 °C for 6 h. After separation, washing, drying and pulverization, carbon nanotubes grafted with polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether were obtained. (3) 20 g of polylactic acid, 2 g of polybutylene adipate terephthalate, 0.2 g of diisopropylbenzene peroxide and 0.5 g of carbon nanotube-grafted polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether were mixed at 165 ℃ for 10 min. The mixed product was crushed, stretched once and stretched twice to obtain antibacterial and antistatic polylactic acid fiber. During the first stretching, the temperatures of each section of the twin-screw extruder were 165 ℃, 175 ℃, 185 ℃ and 175 ℃, the extrusion speed was 0.64 m / min, and the pulling speed was 3.2 m / min. During the second stretching, the heating temperature was 70 ℃, the stretching ratio was 4 times, and the winding speed was 0.5 m / min.

[0021] Example 3 (1) First, 4 g of carbon nanotubes (length 3-12 μm, diameter 8-15 nm) were added to 200 mL of 40% ethanol solution by weight, and ultrasonically dispersed at room temperature for 30 min. Then, 9 g of polydopamine and 0.1 g of tris(hydroxymethyl)aminomethane hydrochloride were added, and magnetic stirring was performed at room temperature for 24 h. After separation, washing, drying, and crushing, polydopamine-modified carbon nanotubes were obtained. (2) Under nitrogen atmosphere, 6 g of polyhexamethylbiguanide hydrochloride was first added to 100 mL of dimethyl sulfoxide, and ultrasonically dispersed at room temperature for 30 min. Then, 4 g of polydopamine-modified carbon nanotubes was added, and magnetic stirring was continued at 60 °C for 10 min. Finally, 12 g of glycerol glycidyl ether was added, and magnetic stirring was continued at 80 °C for 4 h. After separation, washing, drying and pulverization, carbon nanotubes grafted with polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether were obtained. (3) 40 g of polylactic acid, 6 g of poly(butylene adipate terephthalate), 0.8 g of diisopropylbenzene peroxide and 2 g of carbon nanotube-grafted poly(hexamethylbiguanide hydrochloride) bonded with glycerol glycidyl ether were kneaded at 185 ℃ for 6 min. The kneaded product was crushed, stretched once and stretched twice to obtain antibacterial and antistatic polylactic acid fibers. During the first stretching, the temperatures of the twin-screw extruder were 165 ℃, 175 ℃, 185 ℃ and 175 ℃, the extrusion speed was 0.64 m / min, and the pulling speed was 3.2 m / min. During the second stretching, the heating temperature was 90 ℃, the stretching ratio was 6 times, and the winding speed was 1 m / min.

[0022] Comparative Example 1 30 g of polylactic acid and 4 g of polybutylene adipate terephthalate were mixed at 175 ° C for 8 min, and the mixed product was crushed, stretched once, and stretched twice to obtain a finished product; wherein, during the first stretching, the temperatures of each section of the twin-screw extruder were 165 ° C, 175 ° C, 185 ° C and 175 ° C, the extrusion speed was 0.64 m / min, and the pulling speed was 3.2 m / min; the heating temperature during the second stretching was 80 ° C, the stretching multiple was 5 times, and the winding speed was 0.8 m / min.

[0023] Comparative Example 2 30 g of polylactic acid, 4 g of polybutylene adipate terephthalate and 1.2 g of carbon nanotubes (length of 3-12 μm and diameter of 8-15 nm) were mixed at 175 °C for 8 min, and the mixed product was crushed, stretched once and stretched twice to obtain the finished product; wherein, during the first stretching, the temperatures of each section of the twin-screw extruder were 165 °C, 175 °C, 185 °C and 175 °C, the extrusion speed was 0.64 m / min, and the pulling speed was 3.2 m / min; the heating temperature during the second stretching was 80 °C, the stretching ratio was 5 times, and the winding speed was 0.8 m / min.

[0024] Comparative Example 3 30 g of polylactic acid, 4 g of polybutylene adipate terephthalate and 1.2 g of polyhexamethylbiguanide hydrochloride were mixed at 175 °C for 8 min, and the mixed product was crushed, stretched once and stretched twice to obtain a finished product; wherein, during the first stretching, the temperatures of each section of the twin-screw extruder were 165 °C, 175 °C, 185 °C and 175 °C, the extrusion speed was 0.64 m / min, and the pulling speed was 3.2 m / min; the heating temperature during the second stretching was 80 °C, the stretching ratio was 5 times, and the winding speed was 0.8 m / min.

[0025] Comparative Example 4 30 g of polylactic acid, 4 g of polybutylene adipate terephthalate, 0.24 g of carbon nanotubes (length of 3-12 μm, diameter of 8-15 nm) and 0.96 g of polyhexamethylbiguanide hydrochloride were mixed at 175 °C for 8 min, and the mixed product was crushed, stretched once and stretched twice to obtain a finished product; wherein, during the first stretching, the temperatures of each section of the twin-screw extruder were 165 °C, 175 °C, 185 °C and 175 °C, the extrusion speed was 0.64 m / min, and the pulling speed was 3.2 m / min; the heating temperature during the second stretching was 80 °C, the stretching ratio was 5 times, and the winding speed was 0.8 m / min.

[0026] Comparative Example 5 (1) First, 3 g of carbon nanotubes (length 3-12 μm, diameter 8-15 nm) were added to 120 mL of 40% ethanol solution by weight, and ultrasonically dispersed at room temperature for 20 min. Then, 6 g of polydopamine and 0.06 g of tris(hydroxymethyl)aminomethane hydrochloride were added, and magnetic stirring was performed at room temperature for 18 h. After separation, washing, drying and crushing, polydopamine-modified carbon nanotubes were obtained. (2) Under nitrogen atmosphere, 4 g of polyhexamethylbiguanide hydrochloride was first added to 70 mL of dimethyl sulfoxide, and ultrasonically dispersed at room temperature for 20 min. Then, 3 g of polydopamine-modified carbon nanotubes was added, and magnetic stirring was continued at 50 °C for 20 min. Finally, 8 g of glycerol glycidyl ether was added, and magnetic stirring was continued at 70 °C for 5 h. After separation, washing, drying and pulverization, carbon nanotubes grafted with polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether were obtained. (3) 30 g of polylactic acid, 4 g of polybutylene adipate terephthalate and 1.2 g of carbon nanotube-grafted polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether were kneaded at 175 ℃ for 8 min. The kneaded product was crushed, stretched once and stretched twice to obtain a finished product. During the first stretching, the temperatures of each section of the twin-screw extruder were 165 ℃, 175 ℃, 185 ℃ and 175 ℃, the extrusion speed was 0.64 m / min, and the pulling speed was 3.2 m / min. During the second stretching, the heating temperature was 80 ℃, the stretching ratio was 5 times, and the winding speed was 0.8 m / min.

[0027] Comparative Example 6 (1) First, 3 g of carbon nanotubes (length 3-12 μm, diameter 8-15 nm) were added to 120 mL of 40% ethanol solution by weight, and ultrasonically dispersed at room temperature for 20 min. Then, 6 g of polydopamine and 0.06 g of tris(hydroxymethyl)aminomethane hydrochloride were added, and magnetic stirring was performed at room temperature for 18 h. After separation, washing, drying and crushing, polydopamine-modified carbon nanotubes were obtained. (2) Under nitrogen atmosphere, 4 g of polyhexamethylbiguanide hydrochloride was first added to 70 mL of dimethyl sulfoxide, and ultrasonically dispersed at room temperature for 20 min. Then, 3 g of polydopamine-modified carbon nanotubes were added, and magnetic stirring was performed at 50 °C for 20 min. After separation, washing, drying, and crushing, carbon nanotube-grafted polyhexamethylbiguanide hydrochloride was obtained. (3) 30 g of polylactic acid, 4 g of polybutylene adipate terephthalate, 0.5 g of diisopropylbenzene peroxide, 0.6 g of carbon nanotube-grafted polyhexamethylbiguanide hydrochloride and 0.6 g of glycerol glycidyl ether were kneaded at 175 ℃ for 8 min. The kneaded product was crushed, stretched once and stretched twice to obtain a finished product. During the first stretching, the temperatures of the twin-screw extruder were 165 ℃, 175 ℃, 185 ℃ and 175 ℃, the extrusion speed was 0.64 m / min, and the pulling speed was 3.2 m / min. During the second stretching, the heating temperature was 80 ℃, the stretching ratio was 5 times, and the winding speed was 0.8 m / min.

[0028] The diameter of the finished products obtained in the embodiment and the comparative example was tested with a laser diameter gauge, the tensile strength and elongation at break were tested according to GB / T 14337-2022, the resistivity was tested according to GB / T 14342-2015, the antibacterial test was performed according to the oscillation method of GB / T 20944.3-2008, the antibacterial durability was evaluated according to FZ / T 73023-2006, and the antistatic durability was tested according to the literature (Cheng Liang, Jiang Ding, Zhi Jingpeng; Study on the antistatic performance of starch-based composite antistatic agent in polypropylene, China Plastics, 2017, 31(1):25-28). The test results are shown in Table 1.

[0029] Table 1 Performance test results

[0030] It can be seen from the test results that the polylactic acid fibers prepared in the examples have excellent long-term antistatic properties, antibacterial properties and mechanical properties, among which Example 1 has the best effect. In contrast, directly using carbon nanotubes and / or polyhexamethylbiguanide hydrochloride (Comparative Examples 2-4), or using carbon nanotubes grafted with polyhexamethylbiguanide hydrochloride to bond glycerol glycidyl ether without an initiator (Comparative Example 5), or carbon nanotubes grafted with polyhexamethylbiguanide hydrochloride without chemical bonding in advance with glycerol glycidyl ether (Comparative Example 6), polylactic acid fibers with excellent long-term antistatic properties, antibacterial properties and mechanical properties cannot be prepared.

[0031] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A method for preparing antibacterial and antistatic polylactic acid fiber, characterized in that: The polylactic acid fiber is prepared by melt blending, primary drawing and secondary drawing with polylactic acid as a matrix, polybutylene adipate terephthalate as a toughening agent, dicumyl peroxide as an initiator and carbon nanotube grafted polyhexamethylbiguanide hydrochloride bonded glycerol glycidyl ether as an antibacterial and antistatic agent.

2. The method for preparing the antibacterial and antistatic polylactic acid fiber according to claim 1, characterized in that: The specific steps include: (1) First, 2-4 g of carbon nanotubes were added to 50-200 mL of 40% ethanol solution by weight, and ultrasonically dispersed at room temperature for 10-30 min. Then, 3-9 g of polydopamine and 0.02-0.1 g of tris(hydroxymethyl)aminomethane hydrochloride) were added, and magnetic stirring was performed at room temperature for 12-24 h. After separation, washing, drying and crushing, polydopamine-modified carbon nanotubes were obtained. (2) Under nitrogen atmosphere, first add 2-6 g of polyhexamethylbiguanidine hydrochloride into 40-100 mL of dimethyl sulfoxide, and ultrasonically disperse at room temperature for 10-30 min. Then add 2-4 g of polydopamine-modified carbon nanotubes, and magnetically stir at 40-60 °C for 10-30 min. Finally, add 3-12 g of glycerol glycidyl ether, and continue magnetically stirring at 60-80 °C for 4-6 h. After separation, washing, drying and pulverization, carbon nanotubes grafted with polyhexamethylbiguanidine hydrochloride bonded with glycerol glycidyl ether are obtained. (3) According to a certain proportion, polylactic acid, polybutylene adipate terephthalate, diisopropylbenzene peroxide and carbon nanotube grafted polyhexamethylbiguanide hydrochloride bonded with glycerol glycidyl ether are kneaded at 165-185° C. for 6-10 min, and the kneaded product is crushed, stretched once, and stretched twice to obtain the polylactic acid fiber.

3. The method for preparing the antibacterial and antistatic polylactic acid fiber according to claim 2, characterized in that: The carbon nanotubes in step (1) have a length of 3-12 μm and a diameter of 8-15 nm.

4. The method for preparing the antibacterial and antistatic polylactic acid fiber according to claim 2, characterized in that: In parts by weight, the amounts of the materials used in step (3) are: 20-40 parts of polylactic acid, 2-6 parts of polybutylene adipate terephthalate, 0.2-0.8 parts of diisopropylbenzene peroxide, and 0.5-2 parts of carbon nanotube-grafted polyhexamethylbiguanide hydrochloride bonded to glycerol glycidyl ether.

5. The method for preparing the antibacterial and antistatic polylactic acid fiber according to claim 2, characterized in that: The process conditions for the primary stretching in step (3) are as follows: the temperatures of the various sections of the twin-screw extruder are 165°C, 175°C, 185°C and 175°C, the extrusion speed is 0.64 m / min, and the pulling speed is 3.2 m / min.

6. The method for preparing the antibacterial and antistatic polylactic acid fiber according to claim 2, characterized in that: The process conditions of the secondary drawing in step (3) are: heating temperature of 70-90°C, drawing multiple of 4-6 times, and winding speed of 0.5-1 m / min.

7. An antibacterial and antistatic polylactic acid fiber prepared by any method as claimed in any one of claims 1 to 6.