Carbon nano tube / nano silicon composite fiber fabric electrode and preparation method and application thereof
Through the in-situ composite technology and mechanical weaving method of continuous carbon nanotube network and nanosilicon, high-strength, high-conductivity carbon nanotube/nanosi composite fiber fabric electrodes are constructed, and the existing carbon fiber composite electrodes are solved in the field of structural energy storage. The problems of low load capacity and interface instability in the existence of higher energy storage and mechanical properties.
Patent Information
- Application Number
- CN202411139636.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing carbon fiber composite electrodes have a low load of active substances in the field of structural energy storage and the unstable interface structure of the fiber composite electrode, resulting in insufficient specific energy and mechanical bearing capacity of the system, making it difficult to realize a high-strength and high-energy storage structural battery assembly design.
The in-situ continuous composite technology of continuous carbon nanotube network and nanosilicon is adopted to construct carbon nanotube/nanosi composite fiber fabric electrodes through mechanical weaving to achieve high-strength and high-conductivity fiber structure.
It improves the comprehensive performance of multifunctional composite materials, including energy storage capacity and structural mechanical properties, and can effectively improve the electrochemical performance and structural deformation adaptability of lithium-ion batteries. It is suitable for the field of multifunctional structural batteries.
Smart Images

Figure CN119020884A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of negative electrode materials, and specifically relates to a carbon nanotube / nano-silicon composite fiber fabric electrode and a preparation method and application thereof. Background Art
[0002] With the deterioration of the environment and the scarcity of petroleum energy, lightweighting is the direction of future development of new energy battery storage devices. And an effective way to achieve lightweighting is to construct multifunctional composite materials. In recent years, lightweight carbon-based fiber-reinforced composite materials with multifunctionality (taking into account high mechanical strength and good energy storage capacity) have attracted much attention in the field of structural energy storage. For example, carbon fiber reinforced lithium-ion batteries have become the first choice for the integrated design of structural energy storage due to their advantages such as high energy and long life. The structural energy storage currently assembled is mainly divided into two categories: 1) embedded structural energy storage, which mainly embeds a single-function energy storage unit into a carbon fiber reinforced polymer composite laminate or sandwich panel to achieve integrated assembly and design of structural energy storage; 2) composite structural energy storage, such as multifunctional (taking into account structural support and electrode or current collector functions) carbon fiber composite materials.
[0003] Compared with the embedded type, the structure-energy storage integrated design realized by multifunctional composite materials can more effectively reduce the mass of the system and improve the space utilization of the aircraft, thereby further optimizing the overall structure and having higher specific energy and specific strength. However, the electrochemical performance and structural mechanical properties of the battery are highly dependent on the design and assembly of multifunctional composite materials. Therefore, the development and design of new high-performance structural energy storage electrode materials and structural energy storage systems are important research contents. Although composite structural energy storage batteries have made some progress in the past decade, there are still huge challenges in realizing the assembly design of high-strength and high-energy storage structural batteries, especially the design of high-strength and high-energy storage fiber composite electrodes.
[0004] Although the preparation of carbon fiber composite electrodes has been achieved by coating, electrophoretic deposition, vacuum filtration and other methods, the low active material loading and the instability of the fiber composite electrode interface structure reduce the system specific energy and mechanical bearing capacity of the structural battery. In addition, compared with carbon fiber, carbon nanotube fibers with high strength, high toughness and higher conductivity have greater application prospects in the future field of structural energy storage composite material manufacturing. Summary of the invention
[0005] The main purpose of the present invention is to provide a carbon nanotube / nano-silicon composite fiber fabric electrode and a preparation method and application thereof, so as to overcome the deficiencies in the prior art.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0007] The embodiment of the present invention provides a method for preparing a carbon nanotube / nano-silicon composite fiber fabric electrode, which comprises:
[0008] The continuous carbon nanotube network is fully contacted with the nano-silicon dispersion containing nano-silicon, so that the continuous carbon nanotube network and the nano-silicon are continuously and dynamically in-situ uniformly compounded, and simultaneously shrink and fiberize, and the carbon nanotube / nano-silicon composite fiber is obtained by continuous collection, stranding and drying;
[0009] The carbon nanotube / nano-silicon composite fiber is mechanically woven to obtain a carbon nanotube / nano-silicon composite fiber fabric electrode.
[0010] In some embodiments, the carbon nanotube / nano-silicon composite fiber has a diameter of 50-500 μm.
[0011] The embodiment of the present invention also provides a carbon nanotube / nano-silicon composite fiber fabric electrode prepared by the above-mentioned preparation method.
[0012] The embodiment of the present invention also provides the aforementioned carbon nanotube / nano-silicon composite fiber fabric electrode in the field of structural energy storage, preferably as a negative electrode in the preparation of lithium-ion batteries.
[0013] Compared with the prior art, the beneficial effects of the present invention include:
[0014] 1) The preparation method provided by the present invention adopts continuous carbon nanotube network / nano-silicon in-situ continuous composite technology to prepare high-strength carbon nanotube / nano-silicon composite fibers, and realizes the construction of fabric electrodes by means of mechanical weaving; the prepared carbon nanotube / nano-silicon composite fiber fabric electrode can achieve structural optimization through fiber structure and mechanical weaving flexibility, and the fabric electrode can not only be used to assemble traditional lithium-ion batteries such as buttons, soft packs, columns, and flexible batteries, but also can adopt traditional carbon fiber reinforced thermosetting resin curing technology to assemble fiber-reinforced structural lithium-ion batteries that take into account both structural support and energy storage functions, and is used in the field of multifunctional structural batteries;
[0015] 2) In the field of structural lithium-ion batteries, compared with traditional carbon fiber composite electrodes, carbon nanotube / nano-silicon composite fiber fabric electrodes have higher conductivity, electrochemical properties and structural deformation adaptability. When applied to the field of structural energy storage, they can effectively improve the comprehensive performance of multifunctional composite materials, including energy storage and structural mechanical properties (tensile properties, bending properties). BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 is a flow chart for preparing a carbon nanotube / nano-silicon composite fiber fabric electrode in a typical embodiment of the present invention;
[0018] Figure 2a-2c is a photograph of the carbon nanotube / nano-silicon composite fiber prepared in Example 1 of the present invention and a graph showing its tensile and bending resistance;
[0019] Figure 3 is a cross-sectional electron microscope image of the carbon nanotube / nano-silicon composite fiber prepared in Example 1 of the present invention;
[0020] Figure 4 is a tensile curve diagram of the carbon nanotube / nano-silicon composite fiber prepared in Example 1 of the present invention;
[0021] Figure 5 is an electron microscope image of the carbon nanotube / nano-silicon composite fiber fabric electrode prepared in Example 1 of the present invention;
[0022] Figure 6 This is a 0.1A / g constant current charge and discharge curve of the carbon nanotube / nano-silicon composite fiber fabric electrode prepared in Example 1 of the present invention;
[0023] Figure 7 This is a 5A / g constant current charge and discharge curve of the carbon nanotube / nano-silicon composite fiber fabric electrode prepared in Example 1 of the present invention;
[0024] Figure 8 is a cross-sectional electron microscope image of the carbon nanotube / nano-silicon composite fiber prepared in Example 2 of the present invention;
[0025] Fig. 9 is a tensile curve diagram of the carbon nanotube / nano-silicon composite fiber prepared in Example 2 of the present invention;
[0026] Fig.10 is an electron microscope image of the carbon nanotube / nano-silicon composite fiber fabric electrode prepared in Example 2 of the present invention;
[0027] Fig.11 This is a photograph of a structural lithium-ion battery composite plate assembled with carbon nanotube / nano-silicon composite fiber fabric electrodes prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0028] In view of the above-mentioned defects or improvement needs of the prior art, after long-term research and a large number of experiments, the inventors of this case proposed this technical solution, which mainly provides a carbon nanotube / nano-silicon composite fiber fabric electrode and its preparation method and application, and prepares carbon nanotube / nano-silicon composite fibers through a new type of carbon nanotube network and nano-silicon continuous composite technology, and constructs a carbon nanotube / nano-silicon composite fiber fabric electrode with the help of mechanical weaving.
[0029] The technical solution, its implementation process and principle will be further explained as follows.
[0030] As one aspect of the technical solution of the present invention, a method for preparing a carbon nanotube / nano-silicon composite fiber fabric electrode involves:
[0031] The continuous carbon nanotube network is fully contacted with the nano-silicon dispersion containing nano-silicon, so that the continuous carbon nanotube network and the nano-silicon are continuously and dynamically in-situ uniformly compounded, and simultaneously shrink and fiberize, and the carbon nanotube / nano-silicon composite fiber is obtained by continuous collection, stranding and drying;
[0032] The carbon nanotube / nano-silicon composite fiber is mechanically woven to obtain a carbon nanotube / nano-silicon composite fiber fabric electrode.
[0033] In some specific embodiments, the continuous carbon nanotube network is continuously prepared by a floating catalysis method.
[0034] In some specific embodiments, the nano-silicon dispersion comprises nano-silicon, a dispersant, and a solvent.
[0035] Furthermore, the nano-silicon dispersion is prepared by homogenization or ultrasonic process.
[0036] Furthermore, the particle size of the nano-silicon is 20-100 nm.
[0037] Furthermore, the content of nano-silicon in the nano-silicon dispersion is 0.1-0.4 wt %.
[0038] Furthermore, the content of the dispersant in the nano-silicon dispersion is 0.01-0.04 wt %.
[0039] Further, the dispersant may be polyvinyl pyrrolidone (PVP), but is not limited thereto.
[0040] Furthermore, the solvent may include any one or a combination of two or more of ethanol, methanol, dimethylformamide (DMF), dimethylacetamide (DMA), acetonitrile, etc., but is not limited thereto.
[0041] In some specific embodiments, the preparation method includes: continuously and dynamically compounding a continuous carbon nanotube network with nano-silicon in situ and simultaneously shrinking and fiberizing, obtaining single filaments by continuous collection, and then combining and stretching, and drying to obtain carbon nanotube / nano-silicon composite fibers.
[0042] In some specific embodiments, the carbon nanotube / nano-silicon composite fiber is continuously collected at a speed of 1 to 5 m / min.
[0043] Furthermore, the number of the monofilaments to be stranded is 2 to 50 strands.
[0044] Furthermore, the drying includes primary drying before the fiber is rolled up and secondary drying after the fiber is rolled up, wherein the temperature of the quick primary drying before the fiber is rolled up is 80-100°C, and the drying device is dynamic drying during the collection process; the temperature of the secondary drying after the fiber is rolled up is 80-100°C, and the time of the secondary drying is 5-10h.
[0045] In some specific embodiments, the diameter of the carbon nanotube / nano-silicon composite fiber is adjustable, generally 50 to 500 μm.
[0046] In some specific embodiments, the carbon nanotube / nano-silicon composite fiber has excellent tensile properties, with a tensile strength greater than 400 MPa, and can be used as a negative electrode to assemble a high-strength flexible fibrous lithium-ion battery.
[0047] In some specific embodiments, the mechanical weaving method may include plain weaving, twill weaving or 90° weaving, etc.
[0048] In some more preferred embodiments, the method for preparing the carbon nanotube / nanosilicon composite fiber fabric electrode includes the following steps: first, preparing nanosilicon dispersions of different concentrations; then in-situ compounding and synchronous shrinkage fiberization of the continuous carbon nanotube (CNT) network prepared by floating catalysis in the nanosilicon dispersion, utilizing the capillary force between the large-porosity CNT network tubes and their interaction with nanosilicon, through continuous collection, stranding and drying processes, to achieve continuous preparation of carbon nanotube / nanosilicon composite fibers, and through mechanical weaving, controllably constructing the carbon nanotube / nanosilicon composite limited fiber fabric electrode.
[0049] The preparation mechanism of the present invention may be: using a floating catalytic continuous carbon nanotube network as a structural skeleton, with the help of in-situ compounding and fiber shrinkage, to achieve in-situ compounding of nano-silicon, while constructing a long-range ordered, densely oriented carbon nanotube structural skeleton, thereby improving the conductivity, electrochemical properties and tensile and bending resistance of the carbon nanotube / nano-silicon composite fiber; and utilizing the flexibility of mechanical weaving to construct fabric electrodes of different structural models.
[0050] Among them, in some more preferred specific embodiments, please refer to Figure 1 As shown, a method for preparing a carbon nanotube / nano-silicon composite fiber fabric electrode specifically comprises the following steps:
[0051] (1) preparing a nano-silicon dispersion by homogenization or ultrasonic process, wherein the particle size of the nano-silicon is 20 to 100 nm, the content of the nano-silicon is 0.1 to 0.4 wt %, and the content of the dispersant polyvinyl pyrrolidone (PVP) is 0.01 to 0.04 wt %;
[0052] (2) fully contacting the continuous carbon nanotube network prepared by the floating catalytic method with the nano-silicon dispersion, so that the continuous carbon nanotube network and the nano-silicon are continuously and dynamically in-situ uniformly composited and simultaneously shrink and fiberize, and through continuous collection, stranding and drying, the carbon nanotube / nano-silicon composite fiber is obtained;
[0053] (3) Based on carbon nanotube / nano-silicon composite fibers, a carbon nanotube / nano-silicon composite fiber fabric electrode is obtained by mechanical weaving.
[0054] As another aspect of the technical solution of the present invention, it also relates to a carbon nanotube / nano-silicon composite fiber fabric electrode, wherein the fabric electrode is obtained by mechanically weaving the carbon nanotube / nano-silicon composite fibers.
[0055] Furthermore, the diameter of the carbon nanotube / nano-silicon composite fiber is adjustable, specifically 50 to 500 μμm. The nanotube / nano-silicon composite fiber prepared by the present invention has excellent electrical conductivity, tensile properties, mechanical weavability, electrochemical properties, and tensile and bending resistance. Specifically, its electrical conductivity is greater than 500S / cm, and its tensile strength is greater than 400MPa. It can be used as a negative electrode to assemble a high-strength flexible fiber-shaped lithium-ion battery.
[0056] Furthermore, the carbon nanotube / nano-silicon composite fiber fabric electrode exhibits excellent lithium storage performance, with a specific capacity of more than 2500 mAh g -1 .
[0057] Using carbon nanotube / nano-silicon composite fibers as fiber negative electrodes can assemble high-strength, tensile-resistant and flexural-resistant flexible fiber-shaped lithium-ion batteries. In the application of assembling traditional soft-pack or button batteries, compared with traditional thin-film electrodes, the larger gap structure between fibers in the carbon nanotube / nano-silicon composite fiber fabric electrode can provide a path for rapid ion transmission and improve the electrochemical performance of the silicon negative electrode.
[0058] Furthermore, the structural dimensions of the fabric electrode can be controlled by different mechanical weaving models, including plain weaving, twill weaving or 90° weaving.
[0059] Another aspect of the embodiments of the present invention further provides the application of the aforementioned carbon nanotube / nano-silicon composite fiber fabric electrode in the field of lithium-ion batteries, especially in the field of multifunctional structure lithium-ion batteries.
[0060] In some specific embodiments, the carbon nanotube / nano-silicon composite fiber fabric electrode prepared by the present invention can achieve structural optimization through fiber structure and mechanical weaving flexibility, and the fabric electrode can not only be used to assemble traditional lithium-ion batteries such as buttons, soft packs, cylindrical, and flexible batteries, but also can adopt traditional carbon fiber reinforced thermosetting resin curing process to assemble fiber-reinforced structural lithium-ion batteries that take into account both structural support and energy storage functions. It is used in the field of multifunctional structural batteries, providing a new method for designing more flexible and lightweight energy storage systems that take into account both structural support and storage of electrical energy.
[0061] In terms of assembled structural lithium-ion batteries, compared with traditional carbon fiber composite electrodes, carbon nanotube / nano-silicon composite fiber fabric electrodes have higher conductivity, electrochemical properties and structural deformation adaptability. When used in structural energy storage fields such as lithium-ion batteries, they can effectively improve the comprehensive performance of multifunctional composite materials, including energy storage capacity and structural mechanical properties (tensile properties, bending properties, etc.).
[0062] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the embodiments and drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention; all variations associated with or derived from the contents disclosed in the present invention are considered to be within the scope of protection of the present invention.
[0063] The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials involved in the following examples are common commercial products and can be purchased from the market unless otherwise specified.
[0064] The above-mentioned technical features of the present invention and the technical features specifically described below (such as implementation cases) can be combined with each other to form a new or preferred technical solution.
[0065] The raw materials involved in the embodiments of the present invention are either existing commercially available products or can be prepared according to existing methods.
[0066] Example 1
[0067] A method for preparing a carbon nanotube / nano-silicon composite fiber fabric electrode comprises the following specific steps:
[0068] (1) preparing a nano-silicon ethanol dispersion by a homogenization process, wherein the particle size of the nano-silicon is 20 to 100 nm, the content of the nano-silicon is 0.2 wt %, the content of the dispersant polyvinyl pyrrolidone (PVP) is 0.02 wt %, and the solvent is ethanol;
[0069] (2) The continuous carbon nanotube network prepared by the floating catalytic method is fully contacted with the nano-silicon dispersion liquid, so that the continuous carbon nanotube network and the nano-silicon are continuously and dynamically compounded in situ and simultaneously shrink and fiberize, and the carbon nanotube / nano-silicon composite fiber is obtained by continuous collection (collection speed is 2m / min), 10 strands are combined, and drying. The drying process is divided into primary drying and secondary drying. Before the fiber is rolled up, a rapid primary drying is performed at a drying temperature of 80°C; after the fiber is rolled up, a secondary drying is performed at a drying temperature of 80°C and a drying time of 6h; the prepared carbon nanotube / nano-silicon composite fiber has bending resistance (such as Figure 2a-2c ), with a diameter of 100 μm (cross-sectional electron microscopy image as shown in Figure 3 The fiber conductivity is 510S / cm and the tensile strength is about 658MPa (the tensile curve is shown in Figure 4 shown).
[0070] (3) Based on carbon nanotube / nano-silicon composite fibers, carbon nanotube / nano-silicon composite fiber fabric electrodes were obtained by mechanical weaving. The weaving model was plain weave. The electron microscope image of the fabric electrode was as follows: Figure 5 shown.
[0071] A 1cm×1cm fabric electrode was used as the negative electrode, a lithium metal sheet was used as the counter electrode, 1M LiPF6 was dissolved in a mixture of ethylene carbonate (EC) / diethyl carbonate (DEC) / ethyl methyl carbonate (EMC) (1:1:1 by volume), 5.0% fluoroethylene carbonate (FEC) was added as the electrolyte, and a button cell was assembled to detect its specific capacity. The 0.1A / g constant current charge-discharge curve of the fabric electrode is shown in FIG. Figure 6 As shown in the figure, 0.1A / g is as high as 3538mAh / g, showing excellent lithium storage performance. The 5A / g constant current charge and discharge curve of the fabric electrode is shown in the figure Figure 7 As shown, the 5A / g capacity still maintains 1966mAh / g, showing excellent rate performance.
[0072] Example 2
[0073] A method for preparing a carbon nanotube / nano-silicon composite fiber fabric electrode comprises the following specific steps:
[0074] (1) preparing a nano-silicon ethanol dispersion by a homogenization process, wherein the particle size of the nano-silicon is 20 to 100 nm, the content of the nano-silicon is 0.2 wt %, the content of the dispersant polyvinyl pyrrolidone (PVP) is 0.02 wt %, and the solvent is ethanol;
[0075] (2) The continuous carbon nanotube network prepared by the floating catalytic method is fully contacted with the nano-silicon dispersion liquid, so that the continuous carbon nanotube network and the nano-silicon are continuously and dynamically compounded in situ and simultaneously shrink and fiberize, and the carbon nanotube / nano-silicon composite fiber is obtained by continuous collection (collection speed is 5m / min), 30 strands are combined, and drying. Among them, the drying process is divided into primary drying and secondary drying. Before the fiber is rolled up, a rapid primary drying is carried out at a drying temperature of 80°C. After the fiber is rolled up, a secondary drying is carried out at a drying temperature of 80°C and a drying time of 6h. The prepared carbon nanotube / nano-silicon composite fiber has bending resistance and a diameter of 190μm (cross-sectional electron microscope image as shown in FIG. Figure 8 The fiber conductivity is 520S / cm and the tensile strength is about 515MPa (the tensile curve is shown in Fig. 9 shown).
[0076] (3) Based on carbon nanotube / nano-silicon composite fibers, carbon nanotube / nano-silicon composite fiber fabric electrodes were obtained by mechanical weaving. The weaving model was twill. The electron microscope image of the fabric electrode was as follows: Fig.10 shown.
[0077] First, the slurry coating method is used to coat the lithium iron phosphate positive electrode active material on the surface of the carbon fiber fabric, wherein lithium iron phosphate: conductive carbon black: polyvinylidene fluoride = 7:2:1, to prepare a carbon fiber / lithium iron phosphate composite electrode; the solid electrolyte configuration is prepared by using epoxy resin, in combination with lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and ionic liquid 1-ethyl-3-methylimidazole bis(trifluoromethylsulfonyl)imide (EMIM-TFSI), to prepare a dual-continuous phase polymer solid electrolyte with high ionic conductivity and high mechanical strength; the carbon fiber / lithium iron phosphate composite electrode is used as the positive electrode, and the prepared carbon nanotube / nano-silicon composite fiber fabric electrode is used as the negative electrode. The positive and negative electrodes are first soaked in the solid electrolyte and placed between carbon fiber fabrics impregnated with pure epoxy resin. After curing, a structural lithium-ion battery composite plate is obtained, as shown in the photo. Fig.11 As shown, its structure is: 2 layers of carbon fiber fabric impregnated with epoxy / / positive electrode / 1 layer of glass fiber diaphragm impregnated with solid electrolyte / / negative electrode / / 2 layers of carbon fiber fabric impregnated with epoxy. This structure of lithium-ion battery composite plate takes into account both structural support and energy storage performance.
[0078] Example 3
[0079] A method for preparing a carbon nanotube / nano-silicon composite fiber fabric electrode comprises the following specific steps:
[0080] (1) preparing a nano-silicon ethanol dispersion by a homogenization process, wherein the particle size of the nano-silicon is 20 to 100 nm, the content of the nano-silicon is 0.1 wt %, the content of the dispersant polyvinyl pyrrolidone (PVP) is 0.01 wt %, and the solvent is dimethylformamide;
[0081] (2) The continuous carbon nanotube network prepared by the floating catalytic method is fully contacted with the nano-silicon dispersion liquid, so that the continuous carbon nanotube network and the nano-silicon are continuously and dynamically in-situ uniformly compounded, and synchronously shrink and fiberize, and the carbon nanotube / nano-silicon composite fiber is obtained by continuous collection (collection speed is 2m / min), 10 strands are combined, and drying. Among them, the drying process is divided into primary drying and secondary drying. Before the fiber is rolled up, a rapid primary drying is performed, and the drying temperature is 80°C; after the fiber is rolled up, a secondary drying is performed, and the drying temperature is 80°C and the drying time is 6h; the prepared carbon nanotube / nano-silicon composite fiber has bending resistance, a diameter of 102μm, a fiber conductivity of 530S / cm, and a tensile strength of about 659MPa.
[0082] (3) Based on carbon nanotube / nano-silicon composite fibers, a carbon nanotube / nano-silicon composite fiber fabric electrode is obtained by mechanical weaving, and the weaving model is a plain weave.
[0083] A 1cm×1cm fabric electrode was used as the negative electrode and a lithium metal sheet as the counter electrode. 1M LiPF6 was dissolved in a mixture of ethylene carbonate (EC) / diethyl carbonate (DEC) / ethyl methyl carbonate (EMC) (1:1:1 by volume), and 5.0% fluoroethylene carbonate (FEC) was added as the electrolyte. A button battery was assembled and its specific capacity was tested. At 0.1A / g, it was as high as 3501mAh / g, showing excellent lithium storage performance. At 5A / g, the capacity still remained at 1926mAh / g, showing excellent rate performance.
[0084] Example 4
[0085] A method for preparing a carbon nanotube / nano-silicon composite fiber fabric electrode comprises the following specific steps:
[0086] (1) A nano-silicon ethanol dispersion is prepared by a homogenization process, wherein the particle size of the nano-silicon is 20 to 100 nm, the content of the nano-silicon is 0.4 wt %, the content of the dispersant polyvinyl pyrrolidone (PVP) is 0.04 wt %, and the solvent is dimethylacetamide;
[0087] (2) The continuous carbon nanotube network prepared by the floating catalytic method is fully contacted with the nano-silicon dispersion liquid, so that the continuous carbon nanotube network and the nano-silicon are continuously and dynamically in-situ uniformly compounded, and synchronously shrink and fiberize, and the carbon nanotube / nano-silicon composite fiber is obtained by continuous collection (collection speed is 1m / min), 40 strands are combined, and dried. Among them, the drying process is divided into primary drying and secondary drying. Before the fiber is rolled up, a rapid primary drying is performed, and the drying temperature is 80°C; after the fiber is rolled up, a secondary drying is performed, and the drying temperature is 80°C and the drying time is 6h; the prepared carbon nanotube / nano-silicon composite fiber has bending resistance, a diameter of 260μm, a fiber conductivity of 535S / cm, and a tensile strength of about 669MPa.
[0088] (3) Based on carbon nanotube / nano-silicon composite fibers, a carbon nanotube / nano-silicon composite fiber fabric electrode is obtained by mechanical weaving, and the weaving model is twill.
[0089] A 1cm×1cm fabric electrode was used as the negative electrode and a lithium metal sheet as the counter electrode. 1M LiPF6 was dissolved in a mixture of ethylene carbonate (EC) / diethyl carbonate (DEC) / ethyl methyl carbonate (EMC) (1:1:1 by volume). 5.0% fluoroethylene carbonate (FEC) was added as the electrolyte. A button battery was assembled and its specific capacity was tested. The capacity was as high as 3301mAh / g at 0.1A / g, showing excellent lithium storage performance. The capacity remained at 1826mAh / g at 5A / g, showing excellent rate performance.
[0090] In addition, the inventors of this case also conducted experiments with other raw materials and conditions listed in this specification in accordance with the aforementioned embodiments, and also produced a carbon nanotube / nano-silicon composite fiber fabric electrode with excellent conductivity, electrochemical properties and structural deformation adaptability.
[0091] Finally, it should be emphasized that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a carbon nanotube / nano-silicon composite fiber fabric electrode, characterized in that: include: The continuous carbon nanotube network is fully contacted with the nano-silicon dispersion containing nano-silicon, so that the continuous carbon nanotube network and the nano-silicon are continuously and dynamically in-situ uniformly compounded, and simultaneously shrink and fiberize, and the carbon nanotube / nano-silicon composite fiber is obtained by continuous collection, stranding and drying; The carbon nanotube / nano-silicon composite fiber is mechanically woven to obtain a carbon nanotube / nano-silicon composite fiber fabric electrode.
2. The preparation method according to claim 1, characterized in that: The continuous carbon nanotube network is continuously prepared by a floating catalytic method; And / or, the nano-silicon dispersion comprises nano-silicon, a dispersant and a solvent; preferably, the nano-silicon dispersion is prepared by homogenization or ultrasonic process.
3. The preparation method according to claim 2, characterized in that: The particle size of the nano-silicon is 20 to 100 nm; and / or the content of nano-silicon in the nano-silicon dispersion is 0.1 to 0.4 wt %; and / or the content of the dispersant in the nano-silicon dispersion is 0.01 to 0.04 wt %; preferably, the dispersant includes polyvinyl pyrrolidone; and / or the solvent includes any one of ethanol, methanol, dimethylformamide, dimethylacetamide, and acetonitrile, or a combination of two or more thereof.
4. The preparation method according to claim 1, characterized in that: include: The continuous carbon nanotube network and nano-silicon are continuously and dynamically compounded in situ uniformly and contracted synchronously to form fibers. Monofilaments are obtained through continuous collection, and then stranded, stretched and dried to obtain carbon nanotube / nano-silicon composite fibers.
5. The preparation method according to claim 4, characterized in that: The continuous collection speed is 1 to 5 m / min; And / or, the number of the monofilaments to be stranded is 2 to 50; And / or, the drying includes primary drying before fiber winding and secondary drying after fiber winding, wherein the temperature of the primary drying is 80-100°C; the temperature of the secondary drying is 80-100°C, and the time of the secondary drying is 5-10h.
6. The preparation method according to claim 1, characterized in that: The diameter of the carbon nanotube / nano-silicon composite fiber is 50-500 μm; and / or the electrical conductivity of the carbon nanotube / nano-silicon composite fiber is greater than 500 S / cm, and the tensile strength is greater than 400 MPa.
7. The preparation method according to claim 1, characterized in that: The mechanical weaving includes plain weaving, twill weaving or 90° weaving.
8. A carbon nanotube / nano-silicon composite fiber fabric electrode prepared by the preparation method according to any one of claims 1 to 7; preferably, the specific capacity of the carbon nanotube / nano-silicon composite fiber fabric electrode is greater than 2500 mAh g -1 .
9. Use of the carbon nanotube / nano-silicon composite fiber fabric electrode according to claim 8 in the field of structural energy storage, preferably, the application includes use as a negative electrode in the preparation of lithium-ion batteries.
10. The use according to claim 9, characterized in that: The lithium-ion battery includes a multifunctional structure lithium-ion battery. Preferably, the lithium-ion battery includes at least any one of a button lithium-ion battery, a soft-pack lithium-ion battery, a cylindrical lithium-ion battery, a flexible lithium-ion battery, and a fiber-reinforced structure lithium-ion battery.