One-way guiding and absorbing elastic woven fabric capable of being shaped at low temperature

By using polyester/nylon fiber-coated polyolefin yarn in polyester spandex elastic fabric, the core-encapsulated elastic yarn is adopted, and the low-temperature shaping process is used to solve the problem of insufficient soap dipping and color fastness of the fabric at low temperature, and the fabric is realized The excellent elasticity and color fastness are improved, reducing energy consumption and carbon emissions.

CN119020904APending Publication Date: 2024-11-26HUAMAO (XIAMEN) WEAVING DYEING & FINISHING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411348221.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing polypropylene spandex elastic one-way guide wet woven fabric cannot effectively maintain the color and color fastness of the soap liquid during low temperature setting, resulting in the problem of shrinkage and color spitting during the wear and washing process.

Method used

The core-encapsulated elastic yarn is coated with polyolefin yarn through a low-temperature setting process, including warp sizing and shaft weaving, tension-free desizing, dyeing, door Fuji shaping and suction finishing, control temperature and speed, use Moisture-absorbing agent, optimizes the weight percentage of polyolefin elastic yarn and the combination of active groups of resin matrix.

Benefits of technology

It realizes excellent elasticity and elastic recovery of the fabric, improves color fastness, avoids fabric shrinkage and fading problems, reduces energy consumption and carbon emissions, has elastic elongation of more than 20%, and elastic recovery of more than 95%. Dip color/color fastness with soap liquid above level 4.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020904A_ABST
    Figure CN119020904A_ABST
Patent Text Reader

Abstract

The invention discloses a one-way guiding and absorbing elastic woven fabric capable of being shaped at low temperature, and relates to the technical field of textile fabrics. The warp yarns are polyester / nylon fibers or core-spun elastic yarns; the weft yarns are core-spun elastic yarns, polyester / nylon fibers and polypropylene fibers; the core-spun elastic yarn is formed by wrapping polyolefin yarn with polyester / nylon fiber, and the polyolefin yarn accounts for 12-35% of the weight of the core-spun elastic yarn. Wherein the one-way guiding and absorbing elastic woven fabric is composed of a dobby weave, polypropylene fibers are formed on the reverse side, and core-spun elastic yarns are formed on the front side; the method comprises the following steps: step 1, warping, sizing, re-beaming and weaving; step 2, carrying out tension-free desizing; step 3, dyeing; step 4, carrying out centrally-fixed drying; and step 5, suction and discharge arrangement. The one-way absorption guiding elastic woven fabric capable of being shaped at the low temperature has the effects that the elastic elongation is 20% or above, the elastic resilience is 95% or above, and the liquid soap staining / color fastness is level 4 or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of textile fabrics, and in particular to a one-way absorbent stretch woven fabric that can be shaped at low temperatures. Background Art

[0002] One-way moisture conduction technology means that sweat is transferred from the inside of the fabric to the outside of the fabric, while the sweat outside cannot be transferred to the inside of the fabric and is locked to the outer layer, forming a one-way moisture conduction phenomenon. Polypropylene spandex elastic one-way moisture conduction fabric is widely used in outdoor sports, urban leisure and other aspects due to its superior one-way moisture conduction performance.

[0003] In the prior art, polypropylene spandex elastic one-way moisture-conducting woven fabrics have some deficiencies in terms of dyeing and finishing control of fabric elastic width density, etc. Since polypropylene has insufficient high temperature resistance and its melting point is only 165°C, in order to ensure that polypropylene is not melted by high temperature, the setting temperature is generally controlled at around 130°C during dyeing and finishing.

[0004] However, although the setting temperature of 130°C can ensure that polypropylene is not melted by high temperature, it is insufficient for spandex in polypropylene spandex stretch fabrics. In addition, since spandex requires a temperature of 180 to 190°C for high temperature setting, the width cannot be fixed at a setting temperature of 130°C, resulting in the problem of narrow width, heavy weight and excessive elasticity of the fabric. Especially in the process of wearing and washing ready-made clothes, it will also cause the clothes to become longer and longer over time. In order to improve the shrinkage problem of fabrics, the general strategy is to adopt an encrypted method to achieve the shrinkage of fabrics, but this will increase the cost of fabrics and the difficulty of weaving. At the same time, during the dyeing process of the fabric, spandex will absorb the dye, and the dye is only combined with spandex in the form of a physical reaction. Therefore, during the wearing and washing of the fabric, the washing color fastness of the fabric will be affected, especially the water color fastness is the most obvious, causing consumers to often encounter spandex stretch dark clothes and pants after soaking to produce color spitting and light-colored clothes and pants staining, which needs to be improved. Summary of the invention

[0005] In view of this, the purpose of this application is to provide a one-way absorbent stretch woven fabric that can be set at low temperature, which can solve the problem that the existing polypropylene stretch fabric cannot obtain good soap staining or color fastness based on low temperature setting. The specific scheme is as follows:

[0006] A one-way absorbent elastic woven fabric capable of being set at low temperature, comprising warp yarn and weft yarn; the warp yarn is polyester / nylon fiber or core-spun elastic yarn; the weft yarn is core-spun elastic yarn, polyester / nylon fiber and polypropylene; the core-spun elastic yarn is composed of polyester / nylon fiber coated with polyolefin yarn, and the weight percentage of polyolefin yarn in the core-spun elastic yarn is 12-35%; wherein,

[0007] The one-way absorbent stretch woven fabric is composed of a multi-arm structure, and the reverse side is formed with polypropylene and the front side is formed with core-spun stretch yarn;

[0008] And take the following steps:

[0009] Step 1, warping, sizing and weaving: based on the yarn specifications, the warp yarn is free of sizing if it is above 70D, and sizing and waxing is performed if it is below 70D, and the drying temperature of the sizing yarn is controlled to be 140-150℃; the weft yarn is sizing and weaving; finally, the warp yarn and the weft yarn are woven;

[0010] Step 2, tension-free desizing: the fabric obtained by weaving is dyed and finished by direct casting, so that the core-spun stretch yarn can activate the elasticity of the fabric in hot water based on the tension-free desizing and fully shrink in the latter stage;

[0011] Step 3, dyeing: use overflow dyeing machine and control the suction and discharge in the cylinder;

[0012] Step 4: Mid-setting and drying: using Monforts setting machine;

[0013] Step 5: Moisture wicking finishing: Use moisture wicking agents.

[0014] Preferably: the warp yarn is nylon 6ATY 90 / 68FD yarn; the weft yarn includes a first yarn and a second yarn, the first yarn is nylon 6DTY 70D / 68F yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.2, the twist is 800, and the twist direction is Z-direction yarn; the second yarn is white polypropylene DTY 75 / 68SD yarn, and the density is 138 yarns / inch, and the weft density is 148 yarns / inch.

[0015] Preferably: in the warping, sizing and weaving in step 1, the warping machine arranges the warp yarns evenly and forms a whole axis of 1100, sizes the yarns, and then combines them into a weaving axis of 1100*7; the loom adopts a double-nozzle machine, and hangs the first yarn on the first creel, and hangs the second yarn on the second creel, and the rotation speed of the loom is controlled to be 500rpm, and the warp and weft are interwoven in the minimum organizational cycle form of 6*6 coordinates to obtain a first fabric of the first organizational form, wherein the weft directions 1, 2, 3, and 5 are the corresponding core-spun stretch yarns, and 4 and 6 are white polypropylene DTY 75 / 68SD yarns.

[0016] Preferably, the warp yarn is polyester DTY 50 / 72SD yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.0, the twist is 850, and the twist direction is S-direction yarn; the weft yarn includes a third yarn and a fourth yarn, the third yarn is polyester DTY 50 / 72SD yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.0, the twist is 850, and the twist direction is S-direction yarn; the fourth yarn is black polypropylene DTY 75 / 68SD yarn, and the density is 214 yarns / inch, and the weft density is 170 yarns / inch.

[0017] Preferably: in the warping, sizing and weaving of step 1, the warping machine arranges the warp yarns evenly and forms a whole axis 1296, sizes the yarns, and then combines them into a weaving axis 1296*9; the loom adopts a double-nozzle machine, and hangs the third yarn on the third creel, and hangs the fourth yarn on the fourth creel, and controls the rotation speed of the loom to be 450rpm, and interweaves the warp and weft in the minimum organizational cycle form of 4*6 coordinates to obtain a second fabric of the second organizational form, wherein the weft directions 1, 2, 3, and 5 are the corresponding core-spun stretch yarns, and 4 and 6 are black polypropylene DTY 75 / 68SD yarns.

[0018] Preferably: the warp yarn is nylon DTY 20 / 24FD yarn; the weft yarn includes a fifth yarn and a sixth yarn, the fifth yarn is nylon DTY 20 / 24FD yarn and polyolefin stretch yarn, and the draft ratio of the core is 2.8, the twist is 1250, and the twist direction is Z-direction yarn; the sixth yarn is white polypropylene DTY30 / 24SD yarn, and the density is 268 yarns / inch, and the weft density is 178 yarns / inch.

[0019] Preferably: in the warping, sizing and weaving of step 1, the warping machine arranges the warp yarns evenly and forms a whole shaft 1344, sizes the yarns, and then combines them into a weaving shaft 1344*11; the loom adopts a double-nozzle machine, and hangs the fifth yarn on the fifth creel, and hangs the sixth yarn on the sixth creel, and controls the speed of the loom to be 450rpm, and interweaves the warp and weft in the minimum organizational cycle form of 6*12 coordinates to obtain a third fabric with a third organizational form, wherein the weft directions 2, 4, 5, 6, 7, 8, 9, 10, 11, and 12 are the corresponding core-spun stretch yarns, and 1 and 3 are white polypropylene DTY30 / 24SD yarns.

[0020] Preferably: the warp yarn is nylon 6DTY 40 / 34FD yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.0, the twist is 950, and the twist direction is Z-direction yarn; the weft yarn includes a seventh yarn and an eighth yarn, the seventh yarn is nylon 6DTY 40 / 34FD yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.0, the twist is 950, and the twist direction is Z-direction yarn; the eighth yarn is black polypropylene DTY 50 / 48SD yarn, and the density is 195 yarns / inch, and the weft density is 182 yarns / inch.

[0021] Preferably: in the warping, sizing and weaving of step 1, the warping machine arranges the warp yarns evenly and forms a whole axis of 1100, sizes the yarns, and then combines them into a weaving axis of 1100*10; the loom adopts a double-nozzle machine, and hangs the seventh yarn on the seventh creel, and hangs the eighth yarn on the eighth creel, and controls the speed of the loom to be 450rpm, and interweaves the warp and weft in the minimum organizational cycle form of 6*8 coordinates to obtain a fourth fabric with a fourth organizational form, wherein the weft directions 1, 2, 3, 5, 6, and 7 are the corresponding core-spun stretch yarns, and 4 and 8 are black polypropylene DTY 50 / 48SD yarns.

[0022] Preferably: the temperature of the Monfushi setting machine is controlled at 125°C, the speed is 30m / min, and the overfeed is 3-20%; and in the absorption and drainage finishing of step 5, a moisture absorption and perspiration agent is used in the Monfushi setting machine, the temperature is controlled at 125°C, the speed is 30m / min, the overfeed is 3-20%, and then the oven is heat-set for 1.5-3min, and the drying temperature is controlled to 130°C; the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5-2; the first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group; wherein the first active group is an isocyanate group, an acrylamide group, a silane coupling agent, an acyl chloride group or a sulfonic acid group; the second active group is an amino group, a hydroxyl group, a cyano group, an epoxy group, a thiol group or an anhydride group.

[0023] It can be seen from the above scheme that the present application provides a one-way absorbent stretch woven fabric that can be set at low temperature. The one-way absorbent stretch woven fabric that can be set at low temperature is optimized by polyolefin stretch yarn, and the polyolefin stretch yarn is covered with polyester / nylon fiber to avoid the inevitable whitening phenomenon. Based on the characteristic that the polyolefin stretch yarn has a heat setting temperature lower than that of polypropylene, while reducing energy consumption, reducing carbon emissions and carbon footprint, the shrinkage of the fabric is improved and the color fastness is significantly improved. The one-way absorbent stretch woven fabric that can be set at low temperature has excellent elasticity and elastic recovery, and water-washing dimensional stability. At the same time, based on the tests of elastic elongation FZ / T01062-1999, elastic recovery FZ / T01062-1999 and soap staining / color fastness GB / T3921-2008 A, the low-temperature finalizable unidirectional absorbent stretch woven fabric of the present application has an elastic elongation of more than 20%, an elastic recovery of more than 95% and soap staining / color fastness of more than level 4. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0025] Figure 1 This is a schematic diagram of the structure of the first organizational form disclosed in this application;

[0026] Figure 2 A schematic diagram of the structure of the second organizational form disclosed in this application;

[0027] Figure 3 This is a schematic diagram of the structure of the third organizational form disclosed in this application;

[0028] Figure 4 This is a schematic diagram of the structure of the fourth organizational form disclosed in this application. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0030] The following is a detailed description of the low-temperature-setting unidirectional absorbent stretch woven fabric of the present application.

[0031] A unidirectional absorbent stretch woven fabric capable of being set at low temperature comprises warp yarn and weft yarn. The warp yarn is polyester / nylon fiber or core-spun stretch yarn. The weft yarn is core-spun stretch yarn, polyester / nylon fiber and polypropylene.

[0032] It should be mentioned that the core-spun stretch yarn in the embodiment of the present application is composed of polyester / nylon fiber coated polyolefin yarn, and the weight percentage of polyolefin yarn in the core-spun stretch yarn is 12-35%. Among them, the one-way absorbent stretch woven fabric that can be set at low temperature is composed of a multi-arm structure, and polypropylene is formed on the back side, and the core-spun stretch yarn is formed on the front side. Specifically, the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5-2; the first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group; wherein the first active group is an isocyanate group, an acrylamide group, a silane coupling agent, an acyl chloride group or a sulfonic acid group; the second active group is an amino group, a hydroxyl group, a cyano group, an epoxy group, a thiol group or an anhydride group.

[0033] In the preparation process of the low-temperature setting unidirectional absorbent stretch woven fabric, the following steps are adopted:

[0034] Step 1, warping, sizing and weaving: based on the yarn specifications, the warp yarn is free of sizing if it is above 70D, and sizing and waxing is performed if it is below 70D, and the drying temperature of the sizing yarn is controlled to be 140-150℃; the weft yarn is sizing and weaving; finally, the warp yarn and the weft yarn are woven;

[0035] Step 2, tension-free desizing: the fabric obtained by weaving is dyed and finished by direct casting, so that the core-spun stretch yarn can activate the elasticity of the fabric in hot water based on the tension-free desizing and fully shrink in the latter stage;

[0036] Step 3, dyeing: use overflow dyeing machine and control the suction and discharge in the cylinder;

[0037] Step 4: Mid-setting and drying: using Monforts setting machine;

[0038] Step 5: Moisture wicking finishing: Use moisture wicking agents.

[0039] It should be noted that the temperature of the Monfushi setting machine is controlled at 125°C, the speed is 30m / min, and the overfeed is 3-20%. In the absorption and drainage finishing of step 5, a moisture absorption and perspiration wicking agent is used in the Monfushi setting machine, and the temperature is controlled at 125°C, the speed is 30m / min, and the overfeed is 3-20%. Then, the setting is performed in an oven for 1.5-3min, and the drying temperature is controlled at 130°C.

[0040] Embodiment 1

[0041] A unidirectional absorbent elastic woven fabric capable of being set at low temperature comprises warp yarn and weft yarn. The warp yarn is nylon 6ATY90 / 68FD yarn. The weft yarn comprises a first yarn and a second yarn. The first yarn is nylon 6DTY 70D / 68F yarn and polyolefin elastic yarn, and the draft ratio of the core is 3.2, the twist is 800, and the twist direction is Z-direction yarn. The second yarn is white polypropylene DTY 75 / 68SD yarn, and the density is 138 yarns / inch and the weft density is 148 yarns / inch.

[0042] It should be mentioned that the core-spun stretch yarn in the embodiment of the present application is composed of nylon 6DTY 70 / 68FD yarn coated with polyolefin yarn, and the weight percentage of polyolefin yarn in the core-spun stretch yarn is 12%. Among them, the one-way absorbent stretch woven fabric that can be set at low temperature is composed of a multi-arm structure, and polypropylene is formed on the back side, and the core-spun stretch yarn is formed on the front side. Specifically, the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group. The second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is a silane coupling agent. The second active group is a cyano group.

[0043] In the preparation process of the low-temperature setting unidirectional absorbent stretch woven fabric, the following steps are adopted:

[0044] Step 1, warping, sizing and weaving: The warp yarn is based on the yarn specifications. The warp yarn is sizing-free above 70D and sizing and waxing below 70D. The drying temperature of the sizing yarn is controlled to 140°C, and in the first embodiment, it is 75D above 70D. The weft yarn is sizing and weaving, and finally the warp yarn and weft yarn are woven. Specifically, the warping machine arranges the warp yarns evenly and forms a whole shaft 1100, sizes the yarns, and then weaves them into a weaving shaft 1100*7. The loom adopts a double-nozzle machine, and hangs the first yarn on the first creel, and the second yarn on the second creel. The rotation speed of the loom is controlled to 500rpm, such as Figure 1 As shown, the first fabric of the first organizational form is obtained by interweaving the warp and weft in the minimum organizational cycle form of 6*6 coordinates, wherein the weft directions 1, 2, 3, and 5 are corresponding core-spun stretch yarns, and 4 and 6 are white polypropylene DTY 75 / 68SD yarns.

[0045] Step 2, tension-free desizing: the fabric obtained by weaving is dyed and finished by direct casting, so that the core-spun stretch yarn can activate the elasticity of the fabric in hot water based on the tension-free desizing and fully shrink in the latter stage.

[0046] Step 3, dyeing: use overflow dyeing machine and control the suction and discharge in the tank.

[0047] Step 4, mid-setting drying: using a Monforts setting machine, controlling the temperature of the Monforts setting machine to 125°C, the speed to 30m / min, and the overfeed to 8%.

[0048] Step 5, moisture absorption and perspiration finishing: use moisture absorption and perspiration medicaments in a Monforts setting machine, and control the temperature to 125°C, the speed to 30m / min, overfeed 8%, and then heat set in an oven for 1.5min, and control the drying temperature to 130°C.

[0049] Embodiment 2

[0050] A unidirectional absorbent elastic woven fabric capable of being fixed at low temperature comprises warp yarn and weft yarn. The warp yarn is polyester DTY 50 / 72SD yarn and polyolefin elastic yarn, and the draft ratio of the core is 3.0, the twist is 850, and the twist direction is S-direction yarn. The weft yarn comprises a third yarn and a fourth yarn. The third yarn is polyester DTY 50 / 72SD yarn and polyolefin elastic yarn, and the draft ratio of the core is 3.0, the twist is 850, and the twist direction is S-direction yarn. The fourth yarn is black polypropylene DTY 75 / 68SD yarn, and the density is 214 yarns / inch, and the weft density is 170 yarns / inch.

[0051] It should be mentioned that the core-spun stretch yarn in the embodiment of the present application is composed of polyester DTY 50 / 72SD yarn coated with polyolefin yarn, and the weight percentage of polyolefin yarn in the core-spun stretch yarn is 12%. Among them, the one-way absorbent stretch woven fabric that can be set at low temperature is composed of a multi-arm structure, and polypropylene is formed on the back side, and the core-spun stretch yarn is formed on the front side. Specifically, the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group. The second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is a sulfonic acid group. The second active group is an amino group.

[0052] In the preparation process of the low-temperature setting unidirectional absorbent stretch woven fabric, the following steps are adopted:

[0053] Step 1, warping, sizing and weaving: The warp yarn is based on the yarn specifications. The warp yarn is sizing-free above 70D and sizing and waxing is performed below 70D. The drying temperature of the sizing yarn is controlled to 145°C, and in the second embodiment, it is 42D below 70D. The weft yarn is sizing and weaving, and finally the warp yarn and weft yarn are woven. Specifically, the warping machine arranges the warp yarns evenly and forms a whole shaft of 1296, sizes the yarns, and then weaves them into a weaving shaft of 1296*9. The loom adopts a double-nozzle machine, and hangs the third yarn on the third creel, and the fourth yarn on the fourth creel. The rotation speed of the loom is controlled to 450rpm, such as Figure 2As shown, the second fabric of the second organizational form is obtained by interweaving the warp and weft in the minimum organizational cycle form of 4*6 coordinates, wherein the weft directions 1, 2, 3, and 5 are the corresponding core-spun stretch yarns, and 4 and 6 are black polypropylene DTY 75 / 68SD yarns.

[0054] Step 2, tension-free desizing: the fabric obtained by weaving is dyed and finished by direct casting, so that the core-spun stretch yarn can activate the elasticity of the fabric in hot water based on the tension-free desizing and fully shrink in the latter stage;

[0055] Step 3, dyeing: use overflow dyeing machine and control the suction and discharge in the tank.

[0056] Step 4, mid-setting drying: using a Monforts setting machine, controlling the temperature of the Monforts setting machine to 125°C, the speed to 30m / min, and the overfeed to 18%.

[0057] Step 5, moisture absorption and perspiration finishing: use moisture absorption and perspiration medicaments in a Monforts setting machine, and control the temperature to 125°C, the speed to 30m / min, overfeed to 18%, and then heat set in an oven for 2 minutes, and control the drying temperature to 130°C.

[0058] Embodiment 3

[0059] A unidirectional absorbent elastic woven fabric capable of being set at low temperature, comprising warp yarn and weft yarn. The warp yarn is nylon DTY 20 / 24FD yarn. The weft yarn comprises a fifth yarn and a sixth yarn. The fifth yarn is nylon DTY 20 / 24FD yarn and polyolefin elastic yarn, and the draft ratio of the core is 2.8, the twist is 1250, and the twist direction is Z-direction yarn. The sixth yarn is white polypropylene DTY30 / 24SD yarn, and the density is 268 yarns / inch, and the weft density is 178 yarns / inch.

[0060] It should be mentioned that the core-spun stretch yarn in the embodiment of the present application is composed of nylon DTY 20 / 24FD yarn coated with polyolefin yarn, and the weight percentage of polyolefin yarn in the core-spun stretch yarn is 12-35%. Among them, the one-way absorbent stretch woven fabric that can be set at low temperature is composed of a multi-arm structure, and polypropylene is formed on the back side, and the core-spun stretch yarn is formed on the front side. Specifically, the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5-2; the first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group; wherein the first active group is an isocyanate group, an acrylamide group, a silane coupling agent, an acyl chloride group or a sulfonic acid group; the second active group is an amino group, a hydroxyl group, a cyano group, an epoxy group, a thiol group or an anhydride group.

[0061] In the preparation process of the low-temperature setting unidirectional absorbent stretch woven fabric, the following steps are adopted:

[0062] Step 1, warping, sizing and weaving: The warp yarn is based on the yarn specifications. The warp yarn is sizing-free above 70D and sizing and waxing is applied below 70D. The drying temperature of the sizing yarn is controlled to be 150°C, and in the third embodiment, it is 30D below 70D. The weft yarn is sizing and weaving; finally, the warp yarn and the weft yarn are woven. Specifically, the warping machine arranges the warp yarns evenly and forms a whole shaft 1344, sizes the yarns, and then weaves them into a weaving shaft 1344*11. The loom adopts a double-nozzle machine, and hangs the fifth yarn on the fifth creel, and the sixth yarn on the sixth creel. The rotation speed of the loom is controlled to be 450rpm, such as Figure 3 As shown, a third fabric with a third organizational form is obtained by interweaving warp and weft in the minimum organizational cycle form of 6*12 coordinates, wherein the weft directions 2, 4, 5, 6, 7, 8, 9, 10, 11, and 12 are the corresponding core-spun stretch yarns, and 1 and 3 are white polypropylene DTY30 / 24SD yarns.

[0063] Step 2, tension-free desizing: the fabric obtained by weaving is dyed and finished by direct casting, so that the core-spun stretch yarn can activate the elasticity of the fabric in hot water based on the tension-free desizing and fully shrink in the latter stage.

[0064] Step 3, dyeing: use overflow dyeing machine and control the suction and discharge in the tank.

[0065] Step 4, mid-setting drying: using a Monforts setting machine, controlling the temperature of the Monforts setting machine to 125°C, the speed to 30m / min, and the overfeed to 8%.

[0066] Step 5, moisture absorption and perspiration finishing: use moisture absorption and perspiration wicking agent in Monforts setting machine, and control the temperature to 125℃, speed to 30m / min, overfeed 8%, then heat setting in oven for 3min, and control the drying temperature to 130℃.

[0067] Embodiment 4

[0068] A unidirectional absorbent elastic woven fabric capable of being set at low temperature, comprising warp yarn and weft yarn. The warp yarn is nylon 6DTY40 / 34FD yarn and polyolefin elastic yarn, and the draft ratio of the core is 3.0, the twist is 950, and the twist direction is Z-direction yarn. The weft yarn comprises a seventh yarn and an eighth yarn, the seventh yarn is nylon 6DTY 40 / 34FD yarn and polyolefin elastic yarn, and the draft ratio of the core is 3.0, the twist is 950, and the twist direction is Z-direction yarn. The eighth yarn is black polypropylene DTY 50 / 48SD yarn, and the density is 195 yarns / inch, and the weft density is 182 yarns / inch.

[0069] It should be mentioned that the core-spun stretch yarn in the embodiment of the present application is composed of nylon 6DTY 40 / 34FD yarn coated with polyolefin yarn, and the weight percentage of polyolefin yarn in the core-spun stretch yarn is 12-35%. Among them, the one-way absorbent stretch woven fabric that can be set at low temperature is composed of a multi-arm structure, and polypropylene is formed on the back side, and the core-spun stretch yarn is formed on the front side. Specifically, the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group. The second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is a silane coupling agent. The second active group is a cyano group.

[0070] In the preparation process of the low-temperature setting unidirectional absorbent stretch woven fabric, the following steps are adopted:

[0071] Step 1, warping, sizing and weaving: The warp yarn is based on the yarn specifications. The warp yarn is sizing-free above 70D and sizing and waxing is performed below 70D. The drying temperature of the sizing yarn is controlled to be 143°C, and in the fourth embodiment, it is 30D below 70D. The weft yarn is sizing and weaving, and finally the warp yarn and weft yarn are woven. Specifically, the warping machine arranges the warp yarns evenly and forms a whole shaft 1100, sizes the yarns, and then weaves them into a weaving shaft 1100*10. The loom adopts a double-nozzle machine, and hangs the seventh yarn on the seventh creel, and the eighth yarn on the eighth creel. The rotation speed of the loom is controlled to be 450rpm, such as Figure 4 As shown, the fourth fabric of the fourth organizational form is obtained by interweaving the warp and weft in the minimum organizational cycle form of 6*8 coordinates, wherein the weft directions 1, 2, 3, 5, 6, and 7 are the corresponding core-spun stretch yarns, and 4 and 8 are black polypropylene DTY 50 / 48SD yarns.

[0072] Step 2, tension-free desizing: the fabric obtained by weaving is dyed and finished by direct casting, so that the core-spun stretch yarn can activate the elasticity of the fabric in hot water based on the tension-free desizing and fully shrink in the latter stage.

[0073] Step 3, dyeing: use overflow dyeing machine and control the suction and discharge in the tank.

[0074] Step 4, mid-setting drying: using a Monforts setting machine, controlling the temperature of the Monforts setting machine to 125°C, the speed to 30m / min, and the overfeed to 15%.

[0075] Step 5, moisture absorption and perspiration finishing: use moisture absorption and perspiration wicking agent in Monforts setting machine, and control the temperature to 125℃, speed to 30m / min, overfeed to 15%, then heat setting in oven for 3min, and control the drying temperature to 130℃.

[0076] Embodiment 5

[0077] The difference between Example 5 and Example 1 is that the weight percentage of the polyolefin yarn in Example 5 is 23%. The polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:1.4. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is an isocyanate group. The second active group is an anhydride group.

[0078] Embodiment 6

[0079] The difference between Example 6 and Example 1 is that in Example 6, the weight percentage of the polyolefin yarn in the core-spun elastic yarn is 35%. The polyolefin elastic yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:2. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is an acyl chloride group. The second active group is an amino group.

[0080] Embodiment 7

[0081] The difference between Example 7 and Example 2 is that in Example 7, the weight percentage of the polyolefin yarn in the core-spun elastic yarn is 25%. The polyolefin elastic yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:1. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is an acyl chloride group. The second active group is an amino group.

[0082] Embodiment 8

[0083] The difference between Example 8 and Example 2 is that in Example 8, the weight percentage of the polyolefin yarn in the core-spun elastic yarn is 35%. The polyolefin elastic yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:2. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group. The second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is an isocyanate group. The second active group is an anhydride group.

[0084] Embodiment 9

[0085] The difference between Example 9 and Example 3 is that in Example 9, the weight percentage of the polyolefin yarn in the core-spun elastic yarn is 18%. The polyolefin elastic yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:1.5. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group. The second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is an acyl chloride group. The second active group is an epoxy group.

[0086] Embodiment 10

[0087] The difference between Example 10 and Example 3 is that in Example 10, the weight percentage of the polyolefin yarn in the core-spun elastic yarn is 35%. The polyolefin elastic yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:2. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group. The second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is a sulfonic acid group. The second active group is a mercapto group.

[0088] Embodiment 11

[0089] The difference between Example 11 and Example 4 is that in Example 11, the weight percentage of the polyolefin yarn in the core-spun elastic yarn is 27%. The polyolefin elastic yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:1. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group. The second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is an isocyanate group. The second active group is an anhydride group.

[0090] Embodiment 12

[0091] The difference between Example 12 and Example 4 is that in Example 12, the weight percentage of the polyolefin yarn in the core-spun elastic yarn is 35%. The polyolefin elastic yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:2. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group. The second matrix resin is a copolymer of ethylene and butene or octene containing a second active group. Among them, the first active group is an acyl chloride group. The second active group is an amino group.

[0092] Embodiment 13

[0093] The difference between the thirteenth embodiment and the fourth embodiment is that in the step 4 of the thirteenth embodiment, the overfeeding is 20%. In the step 5, the overfeeding is 20%.

[0094] Embodiment 14

[0095] The difference between Example 14 and Example 4 is that the difference between Example 13 and Example 4 in Example 14 is that in Step 4 of Example 13, the overfeeding is 3%. In Step 5, the overfeeding is 3%.

[0096] Comparative Example 1

[0097] The difference between Comparative Example 1 and Example 1 is that the first yarn used for the weft yarn in Comparative Example 1 is nylon 6DTY70 / 48FD and spandex stretch yarn, which are woven to obtain a first comparative grey cloth.

[0098] Comparative Example 2

[0099] The difference between Comparative Example 2 and Example 2 is that the warp yarn and the first weft yarn in Comparative Example 2 are both polyester DTY50 / 72SD and spandex stretch yarn, and the second comparative grey cloth is obtained by weaving.

[0100] Comparative Example 3

[0101] The difference between Comparative Example 3 and Example 1 is that the polyolefin elastic yarn in Comparative Example 3 is polyolefin elastic fiber 75D purchased from Shanghai Liansheng Textile Co., Ltd.

[0102] test:

[0103] 1. Elastic elongation FZ / T01062-1999;

[0104] 2. Elastic recovery FZ / T01062-1999;

[0105] 3. Soap staining / color fastness GB / T3921-2008 A.

[0106] Performance tests were conducted on Examples 1 to 4 and Comparative Examples 1 to 3, and the test results are shown in Table 1 below:

[0107] Table 1 Performance test results

[0108]

[0109] It can be seen from Table 1 above that in the process of drying at 125°C, the width of the obtained one-way absorbent stretch woven fabric is difficult to be shaped according to the set width, resulting in the problem of shrinkage and narrowing. At the same time, compared with comparative example 1, embodiment 1 of the present application and embodiment 2 compared with comparative example 2 have obvious improvements in the direction of elastic elongation, so that the overall elasticity of the obtained one-way absorbent stretch woven fabric is super elastic. In addition, from the aspects of elastic recovery and soap staining / color fastness, it can be seen that the one-way absorbent stretch woven fabric that can be shaped at low temperature in the embodiment of the present application has excellent performance and good soap staining or color fastness under low temperature conditions. Based on the selection of polyolefin stretch yarn, the polyolefin stretch yarn used in the embodiment of the present application is combined with polyester / nylon fiber and polypropylene, so that after low-temperature shaping treatment, the obtained one-way absorbent stretch woven fabric has the effects of avoiding shrinkage, high elasticity and not easy to fade, and can still achieve the purpose of effectively avoiding the problem of fading after continuous use.

[0110] In summary, the present application provides a one-way absorbent stretch woven fabric that can be set at low temperature. The one-way absorbent stretch woven fabric that can be set at low temperature is optimized by polyolefin stretch yarn, and the polyolefin stretch yarn is covered with polyester / nylon fiber to avoid the inevitable whitening phenomenon. Based on the characteristic that the polyolefin stretch yarn has a heat setting temperature lower than that of polypropylene, while reducing energy consumption, reducing carbon emissions and carbon footprint, the shrinkage of the fabric is improved and the color fastness is significantly improved. The one-way absorbent stretch woven fabric that can be set at low temperature has excellent elasticity and elastic recovery, and dimensional stability after washing. At the same time, based on the tests of elastic elongation FZ / T01062-1999, elastic recovery FZ / T01062-1999 and soap staining / color fastness GB / T3921-2008 A, the low-temperature finalizable unidirectional absorbent stretch woven fabric of the present application has an elastic elongation of more than 20%, an elastic recovery of more than 95% and soap staining / color fastness of more than level 4.

[0111] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, or devices.

[0112] It should be noted that the descriptions involving "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0113] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A one-way absorbent stretch woven fabric that can be shaped at low temperature, characterized in that: It includes warp yarn and weft yarn; the warp yarn is polyester / nylon fiber or core-spun stretch yarn; the weft yarn is core-spun stretch yarn, polyester / nylon fiber and polypropylene; the core-spun stretch yarn is composed of polyester / nylon fiber covered with polyolefin yarn, and the weight percentage of polyolefin yarn in the core-spun stretch yarn is 12-35%; wherein, The one-way absorbent stretch woven fabric is composed of a multi-arm structure, and the reverse side is formed with polypropylene and the front side is formed with core-spun stretch yarn; And take the following steps: Step 1, warping, sizing and weaving: based on the yarn specifications, the warp yarn is free of sizing if it is above 70D, and sizing and waxing is performed if it is below 70D, and the drying temperature of the sizing yarn is controlled to be 140-150℃; the weft yarn is sizing and weaving; finally, the warp yarn and the weft yarn are woven; Step 2, tension-free desizing: the fabric obtained by weaving is dyed and finished by direct casting, so that the core-spun stretch yarn can activate the elasticity of the fabric in hot water based on the tension-free desizing and fully shrink in the latter stage; Step 3, dyeing: use overflow dyeing machine and control the suction and discharge in the cylinder; Step 4: Mid-setting and drying: using Monforts setting machine; Step 5: Moisture wicking finishing: Use moisture wicking agents.

2. The low-temperature shaped one-way absorbent stretch woven fabric according to claim 1, characterized in that: The warp yarn is nylon 6ATY 90 / 68FD yarn; the weft yarn includes a first yarn and a second yarn, the first yarn is nylon 6DTY 70D / 68F yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.2, the twist is 800, and the twist direction is Z-direction yarn; the second yarn is white polypropylene DTY 75 / 68SD yarn, and the density is 138 yarns / inch, and the weft density is 148 yarns / inch.

3. The low-temperature shaped one-way absorbent stretch woven fabric according to claim 2, characterized in that: In the warping, sizing and weaving of step 1, the warping machine arranges the warp yarns evenly and forms a whole axis of 1100, sizes the yarns, and then combines them into a weaving axis of 1100*7; the loom adopts a double-nozzle machine, and hangs the first yarn on the first creel, and the second yarn on the second creel, and the rotation speed of the loom is controlled to be 500rpm, and the warp and weft are interwoven in the minimum organizational cycle form of 6*6 coordinates to obtain a first fabric of the first organizational form, wherein the weft directions 1, 2, 3, and 5 are the corresponding core-spun stretch yarns, and 4 and 6 are white polypropylene DTY75 / 68SD yarns.

4. The low-temperature shaped one-way absorbent stretch woven fabric according to claim 1, characterized in that: The warp yarn is polyester DTY 50 / 72SD yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.0, the twist is 850, and the twist direction is S-direction yarn; the weft yarn includes a third yarn and a fourth yarn, the third yarn is polyester DTY 50 / 72SD yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.0, the twist is 850, and the twist direction is S-direction yarn; the fourth yarn is black polypropylene DTY75 / 68SD yarn, and the density is 214 yarns / inch, and the weft density is 170 yarns / inch.

5. The low-temperature shaped one-way absorbent stretch woven fabric according to claim 4, characterized in that: In the warping, sizing and weaving of step 1, the warping machine arranges the warp yarns evenly and forms a whole shaft of 1296, sizes the yarns, and then combines them into a weaving shaft of 1296*9; the loom adopts a double-nozzle machine, and hangs the third yarn on the third creel, and hangs the fourth yarn on the fourth creel, and controls the rotation speed of the loom to be 450rpm, and interweaves the warp and weft in the minimum organizational cycle form of 4*6 coordinates to obtain a second fabric of the second organizational form, wherein the weft directions 1, 2, 3, and 5 are the corresponding core-spun stretch yarns, and 4 and 6 are black polypropylene DTY75 / 68SD yarns.

6. The low-temperature shaped one-way absorbent stretch woven fabric according to claim 1, characterized in that: The warp yarn is nylon DTY 20 / 24FD yarn; the weft yarn includes a fifth yarn and a sixth yarn, the fifth yarn is nylon DTY 20 / 24FD yarn and polyolefin stretch yarn, and the draft ratio of the core is 2.8, the twist is 1250, and the twist direction is Z-direction yarn; the sixth yarn is white polypropylene DTY30 / 24SD yarn, and the density is 268 yarns / inch, and the weft density is 178 yarns / inch.

7. The low-temperature shaped one-way absorbent stretch woven fabric according to claim 6, characterized in that: In the warping, sizing and weaving of step 1, the warping machine arranges the warp yarns evenly and forms a whole shaft 1344, sizes the yarns, and then combines them into a weaving shaft 1344*11; the loom adopts a double-nozzle machine, and hangs the fifth yarn on the fifth creel, and hangs the sixth yarn on the sixth creel, and controls the rotation speed of the loom to be 450rpm, and interweaves the warp and weft in the minimum organizational cycle form of 6*12 coordinates to obtain a third fabric with a third organizational form, wherein the weft directions 2, 4, 5, 6, 7, 8, 9, 10, 11, and 12 are the corresponding core-spun stretch yarns, and 1 and 3 are white polypropylene DTY30 / 24SD yarns.

8. The low-temperature shaped one-way absorbent stretch woven fabric according to claim 1, characterized in that: The warp yarn is nylon 6DTY 40 / 34FD yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.0, the twist is 950, and the twist direction is Z-direction yarn; the weft yarn includes a seventh yarn and an eighth yarn, the seventh yarn is nylon 6DTY 40 / 34FD yarn and polyolefin stretch yarn, and the draft ratio of the core is 3.0, the twist is 950, and the twist direction is Z-direction yarn; the eighth yarn is black polypropylene DTY50 / 48SD yarn, and the density is 195 yarns / inch, and the weft density is 182 yarns / inch.

9. The low-temperature shaped one-way absorbent stretch woven fabric according to claim 8, characterized in that: In the warping, sizing and weaving of step 1, the warping machine arranges the warp yarns evenly and forms a whole axis of 1100, sizes the yarns, and then combines them into a weaving axis of 1100*10; the loom adopts a double-nozzle machine, and hangs the seventh yarn on the seventh creel, and hangs the eighth yarn on the eighth creel, and controls the rotation speed of the loom to be 450rpm, and interweaves the warp and weft in the minimum organizational cycle form of 6*8 coordinates to obtain a fourth fabric of the fourth organizational form, wherein the weft directions 1, 2, 3, 5, 6, and 7 are the corresponding core-spun stretch yarns, and 4 and 8 are black polypropylene DTY 50 / 48SD yarns.

10. A low-temperature shaped one-way absorbent stretch woven fabric according to any one of claims 3, 5, 7 and 9, characterized in that: The temperature of the Monfushi setting machine is controlled at 125°C, the speed is 30m / min, and the overfeed is 3-20%; and in the absorption and discharge finishing of step 5, a moisture absorption and perspiration agent is used in the Monfushi setting machine, the temperature is controlled at 125°C, the speed is 30m / min, the overfeed is 3-20%, and then the oven is heat-set for 1.5-3min, and the drying temperature is controlled to 130°C; the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5-2; the first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group; wherein the first active group is an isocyanate group, an acrylamide group, a silane coupling agent, an acyl chloride group or a sulfonic acid group; the second active group is an amino group, a hydroxyl group, a cyano group, an epoxy group, a thiol group or an anhydride group.

Citation Information

Patent Citations

  • Manufacturing process for low-temperature shaped elastic coating yarn

    CN101200825A

  • Knitted thermal fabric containing both polypropylene and polyolefin elastic fibers

    CN104055231A

  • Low temperature shaping cotton stretch woven fabric and manufacturing method thereof

    CN105986349A

  • Woven fabric with one-way guiding and absorbing function and production technology thereof

    CN107083605A

  • Preparation method of fabric with one-way moisture guiding function

    CN113279107A