High-strength and high-toughness aramid paper and preparation method thereof

By filling the middle layer of aramid paper with floc fibers and glue sealing, combining high-temperature drying and rolling technology, the problem of insufficient strength and toughness of existing aramid paper is solved, and the effect of high strength and high toughness is achieved.

CN119021037APending Publication Date: 2024-11-26NORTH CHINA ELECTRIC POWER UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410236170.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-01
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The middle part of the existing aramid paper is mostly porous, with poor strength, easy to extrude and deform, and relatively poor toughness.

Method used

A middle-layer thickened aramid paper is used, honeycomb holes are installed in the middle and flocculent aramid fiber small pieces are filled with. The flat bottom layer and the surface are bonded and sealed through high-temperature drying and rolling technology to enhance structural stability.

Benefits of technology

By filling the middle-layer thickened aramid paper with floc fibers and glue seals, the strength and toughness of the aramid paper are improved to form a high-strength and high-strength structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119021037A_ABST
    Figure CN119021037A_ABST
Patent Text Reader

Abstract

The high-strength and high-toughness aramid paper comprises middle-layer thickened aramid paper, a flat bottom layer and a flat surface layer, the middle-layer thickened aramid paper is bonded between the flat bottom layer and the flat surface layer, honeycomb holes are formed in the middle of the middle-layer thickened aramid paper, the honeycomb holes are filled with flocculent aramid fiber small blocks, and the flocculent aramid fiber small blocks are arranged in the middle of the middle-layer thickened aramid paper. The thickness of the middle layer thickened aramid paper is 2-8 nm, the thickness of the flat bottom layer is 0.2-0.5 time of the thickness of the middle layer thickened aramid paper, and the thickness of the flat surface layer is 0.1-0.3 time of the thickness of the middle layer thickened aramid paper. The strength of the middle part of the aramid paper is improved, meanwhile, the flocculent aramid fibers have gaps and can be stretched, so that the toughness of the middle part of the aramid paper is enhanced, small flocculent aramid fiber blocks are uniformly distributed in honeycomb holes and are sealed by glue, and the effects of high strength and high toughness are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aramid paper, in particular to high-strength and high-toughness aramid paper and a preparation method thereof. Background Art

[0002] Aramid paper is a special kind of paper made of a synthetic fiber called aramid. There are two types of aramid, one is called meta-aramid, which is aramid 1313, and the other is called para-aramid, which is aramid 1414. Meta-aramid is very resistant to high temperatures, fire, electricity, acid, alkali and radiation, so it can be used for safety protection, high-temperature filtration, electrical insulation, structural materials and other things. Para-aramid is very strong and can withstand great tension and pressure. It can be seen that the application of aramid paper has been very extensive. Aramid paper has multiple structures. The most common ones are honeycomb and composite structure aramid paper.

[0003] However, the aramid paper currently in use has a porous structure in the middle, has poor strength, is easily deformed by extrusion, and has relatively poor toughness. Summary of the invention

[0004] The present invention provides a high-strength and high-toughness aramid paper and a preparation method thereof, which can effectively solve the problems mentioned in the above background technology that the currently used aramid paper has a mostly porous structure in the middle, has poor strength, is easily deformed by extrusion, and has relatively poor toughness.

[0005] To achieve the above object, the present invention provides the following technical solutions: a high-strength and high-toughness aramid paper, comprising a middle layer of thickened aramid paper, a flat bottom layer and a flat surface layer;

[0006] The middle layer of thickened aramid paper is bonded between the flat bottom layer and the flat surface layer;

[0007] The middle part of the middle-layer thickened aramid paper is provided with honeycomb holes, and the honeycomb holes are filled with small pieces of flocculent aramid fibers;

[0008] The thickness of the middle layer thickened aramid paper is 2-8 nm, the thickness of the flat bottom layer is 0.2-0.5 times the thickness of the middle layer thickened aramid paper, and the thickness of the flat surface layer is 0.1-0.3 times the thickness of the middle layer thickened aramid paper.

[0009] According to the above technical solution, the following preparation steps are included:

[0010] S1. Material preparation: first prepare a sufficient amount of aramid base paper, cut part of the aramid base paper into short fibers, prepare precipitated fibers, and prepare several small pieces of flocculent aramid fibers;

[0011] S2, preparation of middle layer thickened aramid paper: firstly, the meta-aramid staple fibers and the precipitated fibers are mixed and stirred, and then sent into a hot press for hot pressing, and then cooled and formed, and then dried and solidified;

[0012] S3, filling flocculent aramid fiber: filling flocculent aramid fiber in the honeycomb holes in the middle of the middle layer thickened aramid paper, and then applying glue on the surface of the middle layer thickened aramid paper to fix it;

[0013] S4. Preparation of a flat bottom layer: several sheets of aramid base paper are coated with glue and stacked together, and then dried at high temperature and squeezed with a long roller at the same time, so that the several sheets of aramid base paper are glued and fixed;

[0014] S5. Preparation of a flat surface layer: several sheets of aramid base paper are coated with glue and stacked together, and then dried at high temperature, and squeezed by a long roller at the same time, so that the several sheets of aramid base paper are glued and fixed;

[0015] S6, Gluing: Apply heated adhesive evenly on both end surfaces of the middle layer thickened aramid paper;

[0016] S7, combined bonding: grinding the sides of the flat bottom layer and the flat surface layer to be bonded, and then bonding the flat bottom layer and the flat surface layer to the two end surfaces of the middle layer thickened aramid paper;

[0017] S8. Uniform rolling: Use a cylinder to roll the bonded aramid paper surface to flatten the surface.

[0018] According to the above technical solution, the volume of the flocculent aramid fiber block in S1 is less than or equal to 1 cm 3 In S2, the internal space of the honeycomb hole in the middle of the middle layer thickened aramid paper is less than or equal to 1 cm 3 .

[0019] According to the above technical solution, in S3, the fibers of the flocculent aramid fiber open the honeycomb holes in the middle of the middle-layer thickened aramid paper, and press the part leaking out of the honeycomb holes, and apply glue to the openings of the honeycomb holes to seal the openings of the honeycomb holes;

[0020] After the glue is applied, let it stand for 10-20 minutes. After the glue is dry, check the coated surface and polish the protruding solidified glue to make the two end surfaces of the middle layer thickened aramid paper smooth.

[0021] According to the above technical solution, in S4 and S5, the flat surface layer and the flat surface layer are covered with glue overflowed by rolling, which is evenly coated on the edge position to wrap the edge gap.

[0022] According to the above technical solution, in S8, during the rolling process, after rolling one side, the reverse side is rolled, and the above operation is repeated 10-20 times.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. By filling the honeycomb holes with small pieces of flocculent aramid fiber and reinforcing the thickened aramid paper in the middle layer, the strength of the middle part of the aramid paper is increased. At the same time, because the flocculent aramid fiber itself has gaps that can be stretched, the toughness of the middle part of the aramid paper is enhanced. The flocculent aramid fiber small pieces are evenly distributed in the honeycomb holes and sealed with glue. The overall structure is stable, achieving the effect of high strength and high toughness.

[0025] 2. By bonding several sheets of aramid paper and rolling them at high temperature, the bonding is even and smooth, and the excess glue can be rolled out, and the overflowed glue is used to bond and seal the edge of the aramid paper to ensure the sealing effect of the edge and efficiently use the glue. Finally, it is bonded to the middle layer of thickened aramid paper to form protection on the outside of the middle layer of thickened aramid paper. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.

[0027] In the attached picture:

[0028] Figure 1 It is a schematic diagram of the structure of the present invention;

[0029] Figure 2 is a flow chart of the steps of the preparation method of the present invention;

[0030] Numbers in the figure: 1. Middle layer of thickened aramid paper; 2. Flat bottom layer; 3. Flat surface layer; 4. Honeycomb holes; 5. Small pieces of flocculent aramid fibers. DETAILED DESCRIPTION

[0031] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0032] Example 1: Figure 1-2 As shown, the present invention provides a technical solution, a high-strength and high-toughness aramid paper, comprising a middle-layer thickened aramid paper 1, a flat bottom layer 2 and a flat surface layer 3;

[0033] The middle layer thickened aramid paper 1 is bonded between the flat bottom layer 2 and the flat surface layer 3;

[0034] A honeycomb hole 4 is arranged in the middle of the middle-layer thickened aramid paper 1, and the honeycomb hole 4 is filled with flocculent aramid fiber small pieces 5;

[0035] The thickness of the middle layer thickened aramid paper 1 is 8 nm, the thickness of the flat bottom layer 2 is 0.5 times the thickness of the middle layer thickened aramid paper 1 , and the thickness of the flat surface layer 3 is 0.3 times the thickness of the middle layer thickened aramid paper 1 .

[0036] The method comprises the following preparation steps:

[0037] S1. Material preparation: first prepare a sufficient amount of aramid base paper, cut part of the aramid base paper into short fibers, prepare precipitated fibers, and prepare a number of flocculent aramid fiber pieces 5;

[0038] S2, preparation of middle layer thickened aramid paper 1: firstly, the meta-aramid staple fibers and the precipitated fibers are mixed and stirred, and then sent into a hot press for hot pressing, and then cooled and formed, and then dried and solidified;

[0039] S3, filling flocculent aramid fiber: filling flocculent aramid fiber in the honeycomb hole 4 in the middle of the middle layer thickened aramid paper 1, and then applying glue on the surface of the middle layer thickened aramid paper 1 to fix it;

[0040] S4, preparation of the flat bottom layer 2: several sheets of aramid base paper are coated with glue and stacked together, and then dried at high temperature, and squeezed by a long roller at the same time, so that the several sheets of aramid base paper are glued and fixed;

[0041] S5, preparation of the flat surface layer 3: several sheets of aramid base paper are coated with glue and stacked together, and then dried at high temperature, and simultaneously squeezed by a long roller, so that the several sheets of aramid base paper are glued and fixed;

[0042] S6, gluing: uniformly coating the heated adhesive on both end surfaces of the middle layer thickened aramid paper 1 in sequence;

[0043] S7, combined bonding: grinding the sides of the flat bottom layer 2 and the flat surface layer 3 to be bonded, and then bonding the flat bottom layer 2 and the flat surface layer 3 to the two end surfaces of the middle layer thickened aramid paper 1;

[0044] S8. Uniform rolling: Use a cylinder to roll the bonded aramid paper surface to flatten the surface.

[0045] The volume of the flocculent aramid fiber block 5 in S1 is 1 cm 3 In S2, the inner space of the honeycomb hole 4 in the middle of the middle layer thickened aramid paper 1 is 1 cm 3 .

[0046] In S3, the fibers of the flocculent aramid fiber open the honeycomb holes 4 in the middle of the middle-layer thickened aramid paper 1, and the part leaking out of the honeycomb holes 4 is pressed, and glue is applied to the openings of the honeycomb holes 4 to seal the openings of the honeycomb holes 4;

[0047] After the glue is applied, let it stand for 20 minutes. After the glue is dried, check the coated surface and polish the protruding solidified glue to make the two end surfaces of the middle layer thickened aramid paper 1 smooth.

[0048] In S4 and S5, the flat surface layer 3 and the flat surface layer 3 are covered with glue overflowed by rolling, and are evenly coated on the edge positions to wrap the edge gaps.

[0049] In S8, during the rolling process, after rolling one side, rolling the reverse side is performed, and the above operation is repeated 20 times.

[0050] Embodiment 2:

[0051] A high-strength and high-toughness aramid paper, comprising a middle-layer thickened aramid paper 1, a flat bottom layer 2 and a flat surface layer 3;

[0052] The middle layer thickened aramid paper 1 is bonded between the flat bottom layer 2 and the flat surface layer 3;

[0053] A honeycomb hole 4 is arranged in the middle of the middle-layer thickened aramid paper 1, and the honeycomb hole 4 is filled with flocculent aramid fiber small pieces 5;

[0054] The thickness of the middle layer thickened aramid paper 1 is 5 nm, the thickness of the flat bottom layer 2 is 0.3 times the thickness of the middle layer thickened aramid paper 1 , and the thickness of the flat surface layer 3 is 0.2 times the thickness of the middle layer thickened aramid paper 1 .

[0055] The method comprises the following preparation steps:

[0056] S1. Material preparation: first prepare a sufficient amount of aramid base paper, cut part of the aramid base paper into short fibers, prepare precipitated fibers, and prepare a number of flocculent aramid fiber pieces 5;

[0057] S2, preparation of middle layer thickened aramid paper 1: firstly, the meta-aramid staple fibers and the precipitated fibers are mixed and stirred, and then sent into a hot press for hot pressing, and then cooled and formed, and then dried and solidified;

[0058] S3, filling flocculent aramid fiber: filling flocculent aramid fiber in the honeycomb hole 4 in the middle of the middle layer thickened aramid paper 1, and then applying glue on the surface of the middle layer thickened aramid paper 1 to fix it;

[0059] S4, preparation of the flat bottom layer 2: several sheets of aramid base paper are coated with glue and stacked together, and then dried at high temperature, and squeezed by a long roller at the same time, so that the several sheets of aramid base paper are glued and fixed;

[0060] S5, preparation of the flat surface layer 3: several sheets of aramid base paper are coated with glue and stacked together, and then dried at high temperature, and simultaneously squeezed by a long roller, so that the several sheets of aramid base paper are glued and fixed;

[0061] S6, gluing: uniformly coating the heated adhesive on both end surfaces of the middle layer thickened aramid paper 1 in sequence;

[0062] S7, combined bonding: grinding the sides of the flat bottom layer 2 and the flat surface layer 3 to be bonded, and then bonding the flat bottom layer 2 and the flat surface layer 3 to the two end surfaces of the middle layer thickened aramid paper 1;

[0063] S8. Uniform rolling: Use a cylinder to roll the bonded aramid paper surface to flatten the surface.

[0064] The volume of the flocculent aramid fiber block 5 in S1 is 0.9 cm 3 In S2, the inner space of the honeycomb hole 4 in the middle of the middle layer thickened aramid paper 1 is 0.9 cm 3 .

[0065] In S3, the fibers of the flocculent aramid fiber open the honeycomb holes 4 in the middle of the middle-layer thickened aramid paper 1, and the part leaking out of the honeycomb holes 4 is pressed, and glue is applied to the openings of the honeycomb holes 4 to seal the openings of the honeycomb holes 4;

[0066] After the glue is applied, let it stand for 15 minutes. After the glue is dried, check the coated surface and polish the protruding solidified glue to make the two end surfaces of the middle layer thickened aramid paper 1 smooth.

[0067] In S4 and S5, the flat surface layer 3 and the flat surface layer 3 are covered with glue overflowed by rolling, and are evenly coated on the edge positions to wrap the edge gaps.

[0068] In S8, during the rolling process, after rolling one side, rolling of the reverse side is performed, and the above operation is repeated 15 times.

[0069] Embodiment 3:

[0070] A high-strength and high-toughness aramid paper, comprising a middle-layer thickened aramid paper 1, a flat bottom layer 2 and a flat surface layer 3;

[0071] The middle layer thickened aramid paper 1 is bonded between the flat bottom layer 2 and the flat surface layer 3;

[0072] A honeycomb hole 4 is arranged in the middle of the middle-layer thickened aramid paper 1, and the honeycomb hole 4 is filled with flocculent aramid fiber small pieces 5;

[0073] The thickness of the middle layer thickened aramid paper 1 is 2 nm, the thickness of the flat bottom layer 2 is 0.2 times the thickness of the middle layer thickened aramid paper 1 , and the thickness of the flat surface layer 3 is 0.1 times the thickness of the middle layer thickened aramid paper 1 .

[0074] The method comprises the following preparation steps:

[0075] S1. Material preparation: first prepare a sufficient amount of aramid base paper, cut part of the aramid base paper into short fibers, prepare precipitated fibers, and prepare a number of flocculent aramid fiber pieces 5;

[0076] S2, preparation of middle layer thickened aramid paper 1: firstly, the meta-aramid staple fibers and the precipitated fibers are mixed and stirred, and then sent into a hot press for hot pressing, and then cooled and formed, and then dried and solidified;

[0077] S3, filling flocculent aramid fiber: filling flocculent aramid fiber in the honeycomb hole 4 in the middle of the middle layer thickened aramid paper 1, and then applying glue on the surface of the middle layer thickened aramid paper 1 to fix it;

[0078] S4, preparation of the flat bottom layer 2: several sheets of aramid base paper are coated with glue and stacked together, and then dried at high temperature, and squeezed by a long roller at the same time, so that the several sheets of aramid base paper are glued and fixed;

[0079] S5, preparation of the flat surface layer 3: several sheets of aramid base paper are coated with glue and stacked together, and then dried at high temperature, and simultaneously squeezed by a long roller, so that the several sheets of aramid base paper are glued and fixed;

[0080] S6, gluing: uniformly coating the heated adhesive on both end surfaces of the middle layer thickened aramid paper 1 in sequence;

[0081] S7, combined bonding: grinding the sides of the flat bottom layer 2 and the flat surface layer 3 to be bonded, and then bonding the flat bottom layer 2 and the flat surface layer 3 to the two end surfaces of the middle layer thickened aramid paper 1;

[0082] S8. Uniform rolling: Use a cylinder to roll the bonded aramid paper surface to flatten the surface.

[0083] The volume of the flocculent aramid fiber block 5 in S1 is 0.5 cm 3 In S2, the inner space of the honeycomb hole 4 in the middle of the middle layer thickened aramid paper 1 is 0.5 cm 3 .

[0084] In S3, the fibers of the flocculent aramid fiber open the honeycomb holes 4 in the middle of the middle-layer thickened aramid paper 1, and the part leaking out of the honeycomb holes 4 is pressed, and glue is applied to the openings of the honeycomb holes 4 to seal the openings of the honeycomb holes 4;

[0085] After the glue is applied, let it stand for 10 minutes. After the glue is dried, check the coated surface and polish the protruding solidified glue to make the two end surfaces of the middle layer thickened aramid paper 1 smooth.

[0086] In S4 and S5, the flat surface layer 3 and the flat surface layer 3 are covered with glue overflowed by rolling, and are evenly coated on the edge positions to wrap the edge gaps.

[0087] In S8, during the rolling process, after rolling one side, rolling the reverse side is performed, and the above operation is repeated 10 times.

[0088] Finally, it should be noted that the above description is only a preferred example of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high-strength and high-toughness aramid paper, characterized in that: It comprises a middle layer of thickened aramid paper (1), a flat bottom layer (2) and a flat surface layer (3); The middle layer of thickened aramid paper (1) is bonded between the flat bottom layer (2) and the flat surface layer (3); The middle portion of the middle layer thickened aramid paper (1) is provided with a honeycomb hole (4), and the honeycomb hole (4) is filled with flocculent aramid fiber small pieces (5); The thickness of the middle layer thickened aramid paper (1) is 2-8 nm, the thickness of the flat bottom layer (2) is 0.2-0.5 times the thickness of the middle layer thickened aramid paper (1), and the thickness of the flat surface layer (3) is 0.1-0.3 times the thickness of the middle layer thickened aramid paper (1).

2. The method for preparing high-strength and high-toughness aramid paper according to claim 1, characterized in that: The method comprises the following preparation steps: S1. Material preparation: first prepare a sufficient amount of aramid base paper, cut part of the aramid base paper into short fibers, prepare precipitated fibers, and prepare a number of flocculent aramid fiber pieces (5); S2, preparation of middle-layer thickened aramid paper (1): firstly, the meta-aramid staple fibers and the precipitated fibers are mixed and stirred, and then sent into a hot press for hot pressing, and then cooled and formed, and then dried and solidified; S3, filling flocculent aramid fibers: filling flocculent aramid fibers in the honeycomb holes (4) in the middle of the middle-layer thickened aramid paper (1), and then applying glue on the surface of the middle-layer thickened aramid paper (1) to fix it; S4, preparation of the flat bottom layer (2): a plurality of aramid base papers are coated with glue and stacked together, and then dried at high temperature and squeezed with a long roller at the same time, so that the plurality of aramid base papers are bonded and fixed to each other; S5, preparation of the flat surface layer (3): a plurality of aramid base papers are coated with glue and stacked together, and then dried at high temperature and squeezed with a long roller at the same time, so that the plurality of aramid base papers are bonded and fixed to each other; S6, gluing: uniformly coating heated adhesive on both end surfaces of the middle layer thickened aramid paper (1); S7, combined bonding: grinding the sides of the flat bottom layer (2) and the flat surface layer (3) to be bonded, and then bonding the flat bottom layer (2) and the flat surface layer (3) to the two end surfaces of the middle layer thickened aramid paper (1); S8. Uniform rolling: Use a cylinder to roll the bonded aramid paper surface to flatten the surface.

3. The method for preparing high-strength and high-toughness aramid paper according to claim 2, characterized in that: The volume of the flocculent aramid fiber block (5) in S1 is less than or equal to 1 cm 3 In said S2, the inner space of the honeycomb hole (4) in the middle of the middle layer thickened aramid paper (1) is less than or equal to 1 cm 3 .

4. The method for preparing high-strength and high-toughness aramid paper according to claim 2, characterized in that: In S3, the fibers of the flocculent aramid fiber open the honeycomb holes (4) in the middle of the middle-layer thickened aramid paper (1), and press the part leaking out of the honeycomb holes (4), and glue is applied to the openings of the honeycomb holes (4) to seal the openings of the honeycomb holes (4); After the glue is applied, it is left to stand for 10-20 minutes. After the glue is dried, the coated surface is checked and the protruding solidified glue is polished to make the two end surfaces of the middle layer thickened aramid paper (1) smooth.

5. The method for preparing high-strength and high-toughness aramid paper according to claim 2, characterized in that: In S4 and S5, the flat surface layer (3) and the flat surface layer (3) are covered with glue overflowed by rolling, and are evenly coated on the edge positions to wrap the edge gaps.

6. The method for preparing high-strength and high-toughness aramid paper according to claim 2, characterized in that: In the above S8, during the rolling process, after rolling one side, rolling the reverse side is performed, and the above operation is repeated 10-20 times.

Citation Information

Patent Citations

  • Hot press molding method of meta-aramid thick paper

    CN110886145A

  • Tensile sound insulation cotton

    CN111038033A

  • Composite material based on honeycomb embedded coupling structure and preparation method thereof

    CN111179896A

  • Reinforced aramid honeycomb sandwich plate

    CN111873558A

  • Novel porous aramid fiber honeycomb filled polymer foaming structure

    CN214084725U