Method for constructing cement-stabilized base by using cement tailings as coarse and fine aggregates

By sorting and screening cement tailings, combining cement, lime and other materials, paving and rolling with specific equipment to form a stable gravel base layer, the problem of pollution and utilization of cement tailings accumulation is solved and high quality is achieved The base material reduces costs and carbon emissions and extends the life of the road.

CN119021053AActive Publication Date: 2024-11-26NO 1 ENG CO LTD OF FHEC OF CCCC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411337737.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-26
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

The storage of cement tailings not only occupies a large amount of land, but also pollutes the environment. It is difficult for the existing technology to effectively utilize it as a stable gravel base material for highways, affecting the environment and engineering quality.

Method used

By conducting preliminary material selection and screening of cement tailings, combining cement, lime and other materials, the particle size ratio and composition ratio are formulated, and equipment such as segregation resistance medium-large pavers, double steel wheel rollers and rubber wheel rollers are used for paving. and roll to form a cement-stabilized gravel base layer and carry out health treatment to ensure the stability and strength of the base layer.

Benefits of technology

The excellent quality of cement tailings as a stable gravel base has been achieved, which reduces production costs, reduces carbon emissions, extends the service life of highways, and improves the utilization rate of waste mineral resources, significantly improving the quality of the project and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to a method for constructing a cement-stabilized gravel base by using cement tailings as coarse and fine aggregates. The method comprises the following steps: batching of a cement-stabilized gravel base, paving of the cement-stabilized gravel base, rolling of the cement-stabilized gravel base, maintenance of the cement-stabilized gravel base and the like. Wherein the particle size ratio of the graded gravel in the cement stabilized gravel lower base layer is (20-31 mm): (10-20 mm): (3-10 mm): (0.075-3 mm) = 18%: 32%: 30%: 20%; wherein the particle size ingredients of the cement tailings respectively account for 6% of 32%, 6% of 30% and 3% of 20% according to the same particle size proportion; the blending proportion of the cement tailings in the cement stabilized base layer replacing the corresponding coarse and fine aggregates in the graded gravel is 15%, the cement tailings and the cement can be used as the stabilized gravel base layer to meet the requirement of excellent quality, and the method has the advantages of simplicity, convenience, practicability, low cost, construction period saving, good quality and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to a method for constructing a water-stable base using cement tailings as coarse and fine aggregates. Background Art

[0002] The highway pavement is composed of 15cm thick crushed stone as the subbase, with a 34cm thick cement-stabilized gravel base on the top of the subbase, and then a total of 19cm thick asphalt surface layers are laid on the top of the cement-stabilized gravel base. The cement-stabilized gravel base serves as a link between the upper and lower layers. The integrity, strength and compaction of the cement-gravel stabilized base play a key role in the quality of the highway.

[0003] Cement tailings are solid materials left over from the limestone beneficiation process, a mixed material with a particle size of 0.075 to 20 mm. Cement tailings are waste materials. Large-scale storage not only occupies a large amount of land and buries plants, but more seriously, the stored cement tailings waste will be discharged into rivers, valleys, and depressions with rainwater, greatly polluting and destroying the human living environment. Therefore, the utilization of cement tailings is an issue that urgently needs to be solved. Summary of the invention

[0004] The purpose of the present invention is to provide a method for constructing a water-stable base using cement tailings as coarse and fine aggregates, which can ensure that the use of cement tailings cement as a stable gravel base meets the requirements of excellent quality, has the advantages of simple and practical method, low cost, saving construction time, good quality and long service life.

[0005] To this end, a method for constructing a water-stable base using cement tailings as coarse and fine aggregates of the present invention comprises the following steps: (1) Select cement tailings, conduct preliminary material selection on the accumulated cement tailings, remove plant weeds, grass roots, and tree roots in the cement tailings, and obtain preliminary material selection of cement tailings; (2) Screening the cement tailings to obtain particle sizes of 0.075-3 mm, 3-10 mm, and 10-20 mm, and storing the particles in different sizes in piles. Spraying water on each pile to moisten its surface, and then covering it with plastic cloth; (3) Ingredients for cement-stabilized gravel base: The cement-stabilized gravel base is divided into a lower base and an upper base. The lower base is located at the lower part of the cement-stabilized gravel base and has a thickness of 21 cm; the upper base is located at the upper part of the cement-stabilized gravel base and has a thickness of 13 cm. (a) The particle size ratio of the intermediate grade gravel in the cement stabilized gravel base is: 20-31mm: 10-20mm: 3-10mm: 0.075-3mm=18%:32%:30%:20%; the particle size ratio of cement tailings is 6% in 32%, 6% in 30%, and 3% in 20% respectively; The weight ratio of each component in the cement-stabilized gravel subbase is: graded gravel: cement: lime = 100: 4.7:1; the maximum dry density is 2.47g / cm 3 , water content 4.6%; (b) The particle size ratio of the intermediate grade gravel in the cement stabilized gravel upper base is: 20-31mm: 10-20mm: 3-10mm: 0.075-3mm=10%:30%:32%:28%; the particle size ratio of cement tailings is 2% in 30%, 8% in 32%, and 5% in 28% respectively; The weight ratio of each component in the cement-stabilized gravel subbase is: graded gravel: cement: lime = 100: 5.1: 0.5; the maximum dry density is 2.43g / cm 3 , water content 4.7%; (4) Paving of cement-stabilized gravel base: divided into upper base and lower base secondary forming paving; (a) The lower base layer is paved in one go with a 21cm thick and full width paving machine using a medium-sized and large anti-segregation paver; once the cement-stabilized gravel lower base layer is paved, the cement-stabilized gravel base layer is rolled immediately, or the paving is completed and followed by rolling. Use a HD130 double-steel-wheel roller to statically roll once at a rolling speed of 1.5 to 1.7 km / h. After ensuring the flatness, use a Yz36 single-steel-wheel roller to vibrate once and use a YL37 rubber-wheel roller to knead once at a rolling speed of 2.0 to 2.5 km / h. (b) Before paving the upper base, spray a layer of cement slurry on the upper end surface of the lower base, and then immediately pave the upper base; the upper base is paved with a thickness of 13 cm and full width in one time using a medium or large anti-segregation paver. Once the paving of the cement-stabilized gravel upper base is completed, the cement-stabilized gravel base is immediately rolled, or the paving is completed and followed by rolling. Use HD130 double steel wheel roller to statically roll once at a speed of 1.5 to 1.7 km / h. After ensuring the flatness, use Yz3 6. Use a single steel wheel roller to vibrate once and use a YL37 rubber wheel roller to roll once, with a rolling speed of 2.0-2.5 km / h; use a Yz36 single steel wheel roller to vibrate and use a YL37 rubber wheel roller to roll, with a rolling speed of 2.0-2.5 km / h to form a combined cycle rolling; the cement stabilized gravel base that has been initially compacted is further rolled in a combined cycle for 4 times to ensure the compaction degree; finally, use a HD130 double steel wheel roller to statically roll for 3 times, with a rolling speed of 2.0-2.5 km / h, and statically press to close the surface; (5) Curing of cement-stabilized gravel base: Once the upper base is rolled, the cement-stabilized gravel base is cured immediately. First, use a sprinkler truck to spray water on the surface of the cement-stabilized gravel base at a rate of 10 to 15 liters / m 2, and then spread the curing film on the surface of the cement-stabilized gravel upper base, and then cover the curing film with geotextile, press environmentally friendly sandbags on the geotextile at intervals, and seal and fix the curing film and geotextile with sandbags around. After a curing period of 5 to 7 days, remove the curing film and geotextile to complete the construction of the water-stabilized base with cement tailings as coarse and fine aggregates.

[0006] As a further description of the above technical solution: the mixing ratio of cement tailings replacing the corresponding coarse and fine aggregates in the graded gravel in the cement stabilized base is 15%.

[0007] As a further description of the above technical solution: in the cement slurry sprayed on the upper end surface of the lower base layer, the weight ratio of cement to water is 10:100.

[0008] As a further description of the above technical solution: the immediately refers to an interval time of less than 5 minutes.

[0009] As a further description of the above technical solution: the cement tailings particle size ingredients must be mixed evenly after being blended with the same particle size ratio.

[0010] As a further description of the above technical solution: the mixing time of the cement tailings as coarse and fine aggregates for the construction of the water-stable base layer is not less than 15 minutes.

[0011] The above method achieves the purpose of the present invention.

[0012] Compared with the prior art, the present invention has the following advantages and positive effects: (1) The present invention can ensure that the use of cement tailings cement as a stabilized gravel base meets the requirements of excellent engineering quality, and has the advantages of simple and practical method, low cost, saving construction time, good quality and long service life. Comparative tests show that the cement stabilized gravel base of the present invention can meet the high-quality engineering quality standards.

[0013] (2) The present invention uses cement tailings instead of coarse and fine aggregates to construct the water-stable base, which can not only reduce production costs, but also reduce carbon emissions, effectively alleviate environmental pressure, and greatly improve the utilization rate of waste mineral resources. Preliminary calculations show that the present invention can save 28% of construction costs and shorten the construction period by 10%, with good economic benefits.

[0014] (3) The present invention significantly reinforces the cement-stabilized gravel base and increases the weight-carrying area, thus significantly extending the service life of the highway. Comparative tests show that the service life of two adjacent sections of highway connected to each other is extended by 2 to 3 times compared with the prior art, and there is no loss, road cracking, collapse, or hollowing. DETAILED DESCRIPTION

[0015] The technical solutions in the embodiments of the present invention are described clearly and completely below. In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments, but the following embodiments are only preferred embodiments of the present invention, not all. Based on the embodiments in the implementation mode, other embodiments obtained by those skilled in the art without creative work all belong to the protection scope of the present invention. The construction methods in the following embodiments are all conventional methods unless otherwise specified, and the materials, devices, equipment, etc. used in the following embodiments are all commercially available unless otherwise specified.

[0016] Embodiment 1: A method for constructing a water-stable base using cement tailings as coarse and fine aggregates, comprising the following steps: (1) Select cement tailings, conduct preliminary material selection on the accumulated cement tailings, remove plant weeds, grass roots, and tree roots in the cement tailings, and obtain preliminary material selection of cement tailings; (2) Screening the cement tailings to obtain particle sizes of 0.075-3 mm, 3-10 mm, and 10-20 mm, and storing the particles in different sizes in piles. Spraying water on each pile to moisten its surface, and then covering it with plastic cloth; (3) Ingredients for cement-stabilized gravel base: The cement-stabilized gravel base is divided into a lower base and an upper base. The lower base is located at the lower part of the cement-stabilized gravel base and has a thickness of 21 cm; the upper base is located at the upper part of the cement-stabilized gravel base and has a thickness of 13 cm. (a) The particle size ratio of the intermediate grade gravel in the cement stabilized gravel base is: 20-31mm: 10-20mm: 3-10mm: 0.075-3mm=18%:32%:30%:20%; the particle size ratio of cement tailings is 6% in 32%, 6% in 30%, and 3% in 20% respectively; The weight ratio of each component in the cement-stabilized gravel subbase is: graded gravel: cement: lime = 100: 4.7:1; the maximum dry density is 2.47g / cm 3 , water content 4.6%; (b) The particle size ratio of the intermediate grade gravel in the cement stabilized gravel upper base is: 20-31mm: 10-20mm: 3-10mm: 0.075-3mm=10%:30%:32%:28%; the particle size ratio of cement tailings is 2% in 30%, 8% in 32%, and 5% in 28% respectively; The mixing ratio of cement tailings replacing the corresponding coarse and fine aggregates in graded gravel in the cement stabilized base is 15%.

[0017] The weight ratio of each component in the cement-stabilized gravel subbase is: graded gravel: cement: lime = 100: 5.1: 0.5; the maximum dry density is 2.43g / cm 3 , water content 4.7%; The cement tailings particle size ingredients must be mixed evenly after being blended with the same particle size ratio. The mixing time of cement tailings as coarse and fine aggregates for the construction of water-stable base paving materials should not be less than 15 minutes.

[0018] (4) Paving of cement-stabilized gravel base: divided into upper base and lower base secondary forming paving; (a) The lower base layer is paved in one go with a 21cm thick and full width paving machine using a medium or large anti-segregation paver. Once the cement-stabilized gravel lower base layer is paved, the cement-stabilized gravel base layer is rolled immediately, or the paving is completed and followed by rolling. Use a HD130 double-steel-wheel roller to roll the surface once at a speed of 1.5 to 1.7 km / h. After ensuring the flatness, use a Yz36 single-steel-wheel roller to vibrate the surface once and use a YL37 rubber-wheel roller to roll the surface once at a speed of 2.0 to 2.5 km / h.

[0019] (b) Before paving the upper base, spray a layer of cement slurry on the upper end of the lower base. The weight ratio of cement to water in the cement slurry is 10:100. Then immediately pave the upper base; the upper base is paved with a medium or large anti-segregation paver to achieve a full thickness of 13cm and full width in one paving. Once the paving of the cement-stabilized gravel upper base is completed, the cement-stabilized gravel base is immediately rolled, or the rolling construction is carried out immediately after the paving is completed. Use HD130 double steel wheel roller to statically roll once, with a rolling speed of 1.5 to 1.7 km / h. After ensuring the flatness, use Yz36 single steel wheel roller to vibrate once and Use YL37 rubber-wheel roller to roll once, with a rolling speed of 2.0-2.5km / h; use Yz36 single steel wheel roller to vibrate and use YL37 rubber wheel roller to roll, with a rolling speed of 2.0-2.5km / h to form a combined cycle rolling; the cement-stabilized gravel base that has been initially rolled is rolled four more times in a combined cycle to ensure the compaction degree; finally, use HD130 double steel wheel roller to roll three times, with a rolling speed of 2.0-2.5km / h, and statically press to finish the surface; (5) Curing of cement-stabilized gravel base: Once the upper base is rolled, the cement-stabilized gravel base is cured immediately. First, use a sprinkler truck to spray water on the surface of the cement-stabilized gravel base at a rate of 10 to 15 liters / m 2, and then spread the curing film on the surface of the cement-stabilized gravel upper base, and then cover the curing film with geotextile, press environmentally friendly sandbags on the geotextile at intervals, and seal and fix the curing film and geotextile with sandbags around. After a curing period of 5 to 7 days, remove the curing film and geotextile, and complete the construction of the water-stabilized base with cement tailings as coarse and fine aggregates. The film and geotextile are products sold on the market.

[0020] Test the cement stabilized gravel base, test the compaction of the cement stabilized gravel base, and handle the unqualified points until they meet the requirements.

[0021] The term "immediately" refers to an interval of less than 5 minutes.

[0022] The test results of the present invention are as follows: (1) The various technical indicators of cement tailings graded gravel have been tested and found to meet the design and specification requirements. The test results are shown in Table 1-1: Table 1-1 Technical indicators of cement tailings graded gravel quality

[0023] (2) Select cement technical indicators. Huaxin or Gezhouba brand cement is selected. After testing, all technical indicators meet the design and specification requirements. The test results are shown in Table 1-2: Table 1-2 Cement quality technical indicators

[0024] (3) The unconfined compressive strength test results of the water-stable base containing 15% cement tailings are shown in Table 1-3 Table 1-3: Unconfined compressive strength test results of tailings water-stable base mixed with 15% cement

[0025] After testing, the unconfined compressive strength test results of the tailings water-stabilized base mixed with 15% cement were found to be in compliance with the design and specification requirements.

[0026] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for constructing a water-stable base using cement tailings as coarse and fine aggregates, characterized in that: The steps include: (1) Select cement tailings, conduct preliminary material selection on the accumulated cement tailings, remove plant weeds, grass roots, and tree roots in the cement tailings, and obtain preliminary material selection of cement tailings; (2) Screening the cement tailings to obtain particle sizes of 0.075-3 mm, 3-10 mm, and 10-20 mm, and storing the particles in different sizes in piles. Spraying water on each pile to moisten its surface, and then covering it with plastic cloth; (3) Ingredients for cement-stabilized gravel base: The cement-stabilized gravel base is divided into a lower base and an upper base. The lower base is located at the lower part of the cement-stabilized gravel base and has a thickness of 21 cm; the upper base is located at the upper part of the cement-stabilized gravel base and has a thickness of 13 cm. (a) The particle size ratio of the intermediate grade gravel in the cement stabilized gravel base is: 20-31mm: 10-20mm: 3-10mm: 0.075-3mm = 18%: 32%: 30%: 20%; the particle size ratio of cement tailings is 6% in 32%, 6% in 30%, and 3% in 20% respectively; The weight ratio of each component in the cement-stabilized gravel subbase is: graded gravel: cement: lime = 100: 4.7:1; the maximum dry density is 2.47g / cm 3 , water content 4.6%; (b) The particle size ratio of the intermediate grade gravel in the cement stabilized gravel upper base is: 20-31mm: 10-20mm: 3-10mm: 0.075-3mm=10%:30%:32%:28%; the particle size ratio of cement tailings is 2% in 30%, 8% in 32%, and 5% in 28% respectively; The weight ratio of each component in the cement-stabilized gravel subbase is: graded gravel: cement: lime = 100: 5.1: 0.5; the maximum dry density is 2.43g / cm 3 , water content 4.7%; (4) Paving of cement-stabilized gravel base: divided into upper base and lower base secondary forming paving; (a) The lower base layer is paved in one go with a 21cm thick and full width paving machine using a medium-sized and large anti-segregation paver; once the cement-stabilized gravel lower base layer is paved, the cement-stabilized gravel base layer is rolled immediately, or the paving is completed and followed by rolling. Use a HD130 double-steel-wheel roller to statically roll once at a rolling speed of 1.5 to 1.7 km / h. After ensuring the flatness, use a Yz36 single-steel-wheel roller to vibrate once and use a YL37 rubber-wheel roller to knead once at a rolling speed of 2.0 to 2.5 km / h. (b) Before paving the upper base, spray a layer of cement slurry on the upper end surface of the lower base, and then immediately pave the upper base; the upper base is paved with a thickness of 13 cm and full width in one time using a medium or large anti-segregation paver. Once the paving of the cement-stabilized gravel upper base is completed, the cement-stabilized gravel base is immediately rolled, or the paving is completed and followed by rolling. Use HD130 double steel wheel roller to statically roll once at a speed of 1.5 to 1.7 km / h. After ensuring the flatness, use Yz3 6. Use a single steel wheel roller to vibrate once and use a YL37 rubber wheel roller to roll once, with a rolling speed of 2.0-2.5 km / h; use a Yz36 single steel wheel roller to vibrate and use a YL37 rubber wheel roller to roll, with a rolling speed of 2.0-2.5 km / h to form a combined cycle rolling; the cement stabilized gravel base that has been initially compacted is further rolled in a combined cycle for 4 times to ensure the compaction degree; finally, use a HD130 double steel wheel roller to statically roll for 3 times, with a rolling speed of 2.0-2.5 km / h, and statically press to close the surface; (5) Curing of cement-stabilized gravel base: Once the upper base is rolled, the cement-stabilized gravel base is cured immediately. First, use a sprinkler truck to spray water on the surface of the cement-stabilized gravel base at a rate of 10 to 15 liters / m 2 , and then spread the curing film on the surface of the cement-stabilized gravel upper base, and then cover the curing film with geotextile, press environmentally friendly sandbags on the geotextile at intervals, and seal and fix the curing film and geotextile with sandbags around. After a curing period of 5 to 7 days, remove the curing film and geotextile to complete the construction of the water-stabilized base with cement tailings as coarse and fine aggregates.

2. The method according to claim 1, characterized in that: The mixing ratio of cement tailings replacing the corresponding coarse and fine aggregates in graded gravel in the cement stabilized base is 15%.

3. The method according to claim 1, characterized in that: A layer of cement slurry is sprayed on the upper end surface of the lower base layer, and the weight ratio of cement to water is 10:

100.

4. The method according to claim 1, characterized in that: The term "immediately" refers to an interval of less than 5 minutes.

5. The method according to claim 1, characterized in that: The cement tailings particle size ingredients must be mixed evenly after being blended with the same particle size ratio.

6. The method according to claim 1, characterized in that: The mixing time of the cement tailings as coarse and fine aggregates for the construction of the water-stable base layer is not less than 15 minutes.

Citation Information

Patent Citations

  • Preparation method of tailing micropowder portland cement

    CN102745919A

  • Construction method of geogrid reinforced clay edge-covered tailing subgrade

    CN104631254A

  • Construction method of cement stabilized gravel base in ultra-high-temperature gale arid area

    CN110904758A

  • Construction method for preventing segregation and reducing cracks of cement stabilized aggregate base layer in low-temperature region

    CN114045729A