Polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder and preparation method thereof

Through the laser melting connection of the polyethylene inner liner and ultra-high molecular weight polyethylene fiber, the difficulty of connecting and recycling of hydrogen cylinders under high pressure is solved, and the cost-effective production and environmentally friendly utilization of hydrogen cylinders are achieved.

CN119022213APending Publication Date: 2024-11-26ZHEJIANG ROTOUN PLASTIC TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411215397.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

When existing hydrogen cylinders are used under high pressure, it is difficult to connect carbon fiber to plastic inner vessels, and carbon fiber is costly and has low recycling value, resulting in environmental protection problems.

Method used

The polyethylene inner liner is wound with ultra-high molecular weight polyethylene fibers to form a fiber protective layer, and is connected to pretension through laser melting to form a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder.

Benefits of technology

It realizes efficient connection of polyethylene materials, reduces production costs, improves the pressure resistance of hydrogen cylinders, and because the materials are exactly the same, it is convenient for recycling and utilization and avoids waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119022213A_ABST
    Figure CN119022213A_ABST
Patent Text Reader

Abstract

According to the polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder and the preparation method thereof, a polyethylene inner container is obtained through rotational molding and used for containing hydrogen to serve as a gas barrier. The ultra-high molecular weight polyethylene fibers are wound on the outer side of the polyethylene inner container to form a fiber protection layer, the polyethylene inner container is surrounded by the fiber protection layer, the polyethylene inner container is protected, and meanwhile certain pressure resistance is achieved. Laser irradiates the fiber protection layer and the polyethylene inner container to melt the fiber protection layer and the polyethylene inner container and are connected into a whole through pretension. Firstly, the polyethylene inner container and the fiber protection layer made of the ultra-high molecular weight polyethylene fibers are connected into a whole through a laser curing method, and the method is simple, safe and convenient to implement; secondly, the ultra-high molecular weight polyethylene fiber is used, so that the strength is high, the weight is light, the price is economical, and large-batch production is facilitated; and finally, the polyethylene inner container and the ultra-high molecular weight polyethylene fiber are both made of polyethylene essentially and can be recycled, so that the device is more economical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-pressure containers, and in particular to a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder and a preparation method thereof. Background Art

[0002] At present, the mainstream process for making hydrogen cylinders is to use polyethylene, nylon or thermoplastics to make the inner liner, and then wrap it with carbon fiber to withstand the pressure. Because the hydrogen cylinder has to withstand a pressure of 700 atmospheres, the carbon fiber is cured with epoxy resin while heating to form a thermosetting composite material layer of epoxy resin and carbon fiber. This method has the following problems: The connection between the plastic liner and the carbon fiber composite layer is difficult. For example, in large hydrogen cylinders of hundreds or even thousands of liters, the peeling between the carbon fiber layer and the plastic layer becomes a very fatal problem.

[0003] In addition, there is the problem of foreign technology restrictions on carbon fiber. Hydrogen cylinders withstand 700 atmospheres of pressure, which requires the strength of carbon fiber to be above T700. This high-strength carbon fiber is expensive and cannot be reliably operated commercially on a large scale.

[0004] Hydrogen cylinders are mainly used in vehicles. All vehicles have a lifespan and must be scrapped when the time comes. Generally, carbon fiber hydrogen cylinders will also be scrapped at that time. Hydrogen cylinders are made of a composite of multiple materials, and the carbon fiber on the outside is a thermosetting material. Therefore, once it is scrapped in the future, it will have no recycling value at all, causing huge environmental problems.

[0005] Therefore, the problems existing in the prior art need to be further improved and developed. Summary of the invention

[0006] (I) Purpose of the invention: In order to solve the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder and a preparation method thereof.

[0007] (II) Technical solution: In order to solve the above technical problems, the present technical solution provides a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder, comprising a polyethylene liner and a fiber protective layer formed by winding ultra-high molecular weight polyethylene fibers; the polyethylene liner contains hydrogen and serves as a gas barrier; The polyethylene liner is cylindrical, and is provided with arc-shaped interfaces at both ends, wherein the arc-shaped interfaces include a seat opening connected to the valve seat and an arc-shaped surface located at the edge of the seat opening; a valve seat is provided on the outer side of the arc-shaped interface, and sealing is performed through the valve seat; The fiber protective layer serves as a load-bearing structure, surrounding the polyethylene inner liner inside, thereby protecting the polyethylene inner liner and having a certain pressure resistance.

[0008] Preferably, the wall thickness of the polyethylene liner is in the range of 5 mm to 20 mm; and the ratio of the length to the inner diameter of the polyethylene liner is in the range of 4:1 to 5:1.

[0009] Preferably, the polyethylene liner has a surface melting zone, and the fiber protective layer has a laser slit zone in a region corresponding to the surface melting zone; the surface melting zone and / or the laser slit zone are arranged along the axial direction of the polyethylene liner and / or the fiber protective layer, and are equal in length to the polyethylene liner and the fiber protective layer; The surface melting zone and the laser slit zone are adhered to connect the polyethylene liner and the fiber protective layer into a whole.

[0010] A method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder, used for preparing the polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder, comprises the following steps: Step 1, obtaining a polyethylene liner by rotational molding; Step 2, winding ultra-high molecular weight polyethylene fiber on the outside of the polyethylene liner to form a fiber protective layer; Step 3: Laser irradiates the fiber protective layer and the polyethylene liner to melt the two, and connect them into one through pre-tension.

[0011] Preferably, the step 1 specifically includes: Step 101, applying a release agent on each component of the molding die, and assembling the coated molding die components to obtain a molding die; Step 102, adding polyethylene raw material into the molding die and installing it on a rotating machine; Step 103, heating the molding die and rotating it around a rotation axis; Step 104, cooling and demoulding to obtain a polyethylene liner.

[0012] Preferably, the rotating machine has a rotatable main shaft fixed arm and an adjustment disk as a secondary shaft, the molding die is placed horizontally with the rotation center and the swing center in the horizontal direction, and the center of the liner coincides with the rotation center and the swing center; The rotation speed of the fixed arm is called the arm speed, the rotation speed of the adjusting disk is called the disk speed, and the arm speed is divided by the difference between the disk speed and the arm speed as the speed ratio; under the condition of ensuring that the speed ratio range is less than 1:2, a swing rotating machine is used for production and manufacturing, and then annealing and cooling are performed to obtain an inner liner with a flat inner surface.

[0013] Preferably, the molding die rotates around the axis at a speed of 1 r / min, the swing angle is ±45°, the limit position dwell time is 0 s, and the swing speed is 6.5 times / min. At this time, the wall thickness tolerance of the polyethylene liner is controlled at 5.89 mm ± 0.53 mm.

[0014] Preferably, the step 3 is specifically: Step 301, irradiating the fiber protective layer with a laser to melt the ultra-high molecular weight polyethylene fiber; Step 302, irradiating the polyethylene liner with a laser to melt the surface of the polyethylene liner; Step 303: Connect the fiber protective layer and the polyethylene liner by pre-tensioning to obtain a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder.

[0015] Preferably, a laser path is formed on the fiber protective layer by laser irradiation, and the heat generated by the laser melts the ultra-high molecular weight polyethylene fibers in the laser path area to generate a laser slit band; The laser temperature reaches 150° C.; and the laser irradiation time is less than or equal to 3 seconds.

[0016] Preferably, a laser is used to irradiate the polyethylene liner area corresponding to the laser slit band on the fiber protective layer, and the heat generated by the laser melts the surface of the polyethylene liner to produce a surface melting band; The moving speed of the laser irradiating the polyethylene liner should be increased by 10% to 50% compared with the moving speed of the laser irradiating the ultra-high molecular weight polyethylene fiber.

[0017] (III) Beneficial effects: The present invention provides a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder and a preparation method thereof. First, the polyethylene liner and the fiber protective layer of the ultra-high molecular weight polyethylene fiber are connected as one by laser curing. The method is simple, safe and easy to implement. Secondly, the ultra-high molecular weight polyethylene fiber is used, which has high strength, light weight, economical price and is convenient for mass production. Finally, the polyethylene liner and the ultra-high molecular weight polyethylene fiber are both polyethylene in essence. Therefore, the obtained hydrogen cylinder is made entirely of polyethylene material, which can be recycled, avoiding the problem of waste and being more economical. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a structural diagram of a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder of the present invention; Figure 2 This is a flow chart of a method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder of the present invention; Figure 3 This is a flow chart of the method for preparing a polyethylene liner of the present invention; Figure 4 It is a detailed flow chart of the laser curing of the present invention. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below in conjunction with preferred embodiments. More details are elaborated in the following description to facilitate a full understanding of the present invention. However, the present invention can obviously be implemented in a variety of other ways different from the description. Those skilled in the art can make similar generalizations and deductions based on actual application situations without violating the connotation of the present invention. Therefore, the protection scope of the present invention should not be limited by the content of this specific embodiment.

[0020] The accompanying drawings are schematic diagrams of embodiments of the present invention. It should be noted that the drawings are only examples and are not drawn to scale, and should not be used to limit the actual protection scope of the present invention.

[0021] A polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder, such as Figure 1 As shown, it includes a polyethylene liner 1 and a fiber protective layer 2 formed by winding ultra-high molecular weight polyethylene fibers. The polyethylene liner 1 contains hydrogen and serves as a gas barrier; the fiber protective layer 2 serves as a load-bearing structure, surrounding the polyethylene liner 1 inside, protecting the polyethylene liner 1 and having a certain pressure resistance.

[0022] The polyethylene liner 1 includes the following four models: diameter 140mm, height 870mm, volume 10L, maximum working pressure 30MPa; diameter 159mm, height 1100mm, volume 20L, maximum working pressure 30MPa; diameter 219mm, height 1380mm, volume 40L, maximum working pressure 30MPa; diameter 219mm, height 1680mm, volume 50L, maximum working pressure 30MPa. It should be noted that no matter which model of polyethylene liner 1, the wall thickness of the polyethylene liner 1 of the present invention ranges from 5mm to 20mm.

[0023] The polyethylene liner 1 is cylindrical, and is provided with arc-shaped interfaces at both ends, wherein the arc-shaped interfaces include a seat opening connected to a valve seat and an arc-shaped surface located at the edge of the seat opening. A valve seat is provided on the outside of the arc-shaped interface, and the polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder is sealed by the valve seat.

[0024] The ratio of the length to the inner diameter of the polyethylene liner 1 described in the present invention is in the range of 4:1 to 5:1. The arc-shaped interface is a dome-shaped curved surface. The valve seat is a metal valve seat, which can be made of materials with good ductility and strong corrosion resistance such as aluminum alloy and Austrian stainless steel, and the specific material is not limited. The connection between the arc-shaped interface and the valve seat can be a through hole or a blind hole, which is not required in the present invention.

[0025] The polyethylene liner 1 has a surface melting zone, and the fiber protective layer 2 has a laser slit zone in the area corresponding to the surface melting zone. The surface melting zone and the laser slit zone are adhered to connect the polyethylene liner 1 and the fiber protective layer 2 into a whole, thereby obtaining a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder.

[0026] The surface melting zone and / or the laser slit zone are arranged along the axial direction of the polyethylene liner 1 and / or the fiber protective layer 2, that is, perpendicular to the circumferential direction of the polyethylene liner 1 and / or the fiber protective layer 2; extending from the valve seat at one end to the valve seat at the other end, and having the same length as the polyethylene liner 1 and the fiber protective layer 2. The position of the surface melting zone and / or the laser slit zone in the circumferential direction of the polyethylene liner 1 and / or the fiber protective layer 2 is not limited, as long as the two are corresponding to each other so as to be connected into a whole.

[0027] The height of the fiber protective layer 2 changes with the height of the polyethylene liner 1, and the thickness of the fiber protective layer 2 remains the same. That is, when the model of the polyethylene liner 1 is 140 mm in diameter, 870 mm in height, and 10 L in volume, and when the model of the polyethylene liner 1 is 219 mm in diameter, 1680 mm in height, and 50 L in volume, the thickness of the fiber protective layer 2 is equal, and the length remains the same as the length of the polyethylene liner 1.

[0028] A method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder, used for preparing the polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder, such as Figure 2 As shown, the following steps are included: Step 1: obtain a polyethylene liner by rotational molding.

[0029] Step 2: Wrap ultra-high molecular weight polyethylene fiber around the outside of the polyethylene liner to form a fiber protective layer.

[0030] Step 3: Laser irradiates the fiber protective layer and the polyethylene liner to melt the two, and connect them into one through pre-tension.

[0031] More specifically, Figure 3 As shown, the step 1 specifically includes: Step 101: Apply a release agent to each component of a molding die, and assemble the coated molding die components to obtain a molding die.

[0032] The molding die includes the mold of the polyethylene liner 1 and the valve seats at both ends of the polyethylene liner 1, and the various parts of the molding die are assembled, including but not limited to half molds, inserts, molding accessories, etc. The half molds are spliced ​​to form the molding die; the inserts mainly play the role of local reinforcement parts; the molding accessories are mainly modules for ribbing or special parts molding.

[0033] The purpose of applying the release agent on the components of the molding mold is to facilitate the removal of the molded polyethylene liner from the molding mold, and at the same time, it can effectively avoid the phenomenon that the polyethylene liner is damaged during demoulding due to the strong adhesion between the polyethylene liner and the components of the molding mold.

[0034] The release agent can be a fluorine release agent or a silicone release agent. The fluorine release agent has excellent isolation performance and low pollution to the mold, but the cost is relatively high. The silicone release agent has good isolation performance and low pollution to the mold, and can be used multiple times after being applied once. Silicone oil is usually mixed with organic solvents such as toluene; silicone oil has a good demoulding effect and little pollution to the mold.

[0035] Step 102: Add polyethylene raw material into the molding die and install it on a rotating machine.

[0036] Accurately weigh the weight of the polyethylene raw material required for the polyethylene liner, add the weighed polyethylene raw material to the bottom of one of the half molds of the molding mold, remove the remaining polyethylene raw material at the mold joint of the two half molds, ensure that the two half molds are tightly fitted at the parting surface to avoid leakage of the polyethylene raw material during processing, and then tighten the two half molds together and install them on the rotating shaft.

[0037] Step 103: heating the molding die and rotating the die around the rotation axis.

[0038] The molding die is mounted on a rotating machine, the molding die is rotated, and the molding die is heated at the same time. The polyethylene raw material gradually melts under the rotation and heating, and is deposited on the entire inner wall of the mold cavity of the molding die. The gas contained in the polyethylene raw material is gradually removed, and a well-molded polyethylene liner is obtained.

[0039] The heating may be performed by placing the molding die into a heating furnace, or by heating with a heat source such as gas or flame, which is not specifically limited herein. The molding die is heated to ensure that the temperature reaches 230°C to 350°C, and the more preferred temperature is 320°C.

[0040] The rotary machine has a rotatable main shaft fixed arm and an adjustment disk as a secondary shaft, including an L-arm rotary machine, a straight arm rotary machine and a swing rotary machine, wherein the rotation center of the fixed arm of the L-arm rotary machine does not coincide with the horizontal center of the adjustment disk, the rotation center of the fixed arm of the straight arm rotary machine does not coincide with the horizontal center of the adjustment disk, and the swing rotary machine adds a swing function on the basis of the L-arm rotary machine or the straight arm rotary machine. This embodiment uses a swing rotary machine, the molding mold is placed horizontally with the rotation center and the swing center in the horizontal direction, and the center of the inner liner coincides with the rotation center and the swing center.

[0041] The rotation speed of the fixed arm is called the arm speed, the rotation speed of the adjustment disk is called the disk speed, and the arm speed is divided by the difference between the disk speed and the arm speed as the speed ratio. The uniformity of the wall thickness of the polyethylene liner 1 can be adjusted by adjusting the speed ratio. In this embodiment, a swinging rotary machine is used for production and manufacturing under the condition of ensuring that the speed ratio range is less than 1:2, and then annealing and cooling are performed to obtain an liner with a flat inner surface.

[0042] More specifically, the rotation speed of the molding die around the axis is set to 1r / min, the swing angle is ±45°, the limit position dwell time is 0s, and the swing speed is 6.5 times / min. At this time, the standard deviation of the wall thickness of the polyethylene liner obtained by the molding die has a minimum value of 0.178. According to the normal distribution 3σ principle, the wall thickness tolerance of the polyethylene liner can be controlled at 5.89mm±0.53mm at this time, so the wall thickness uniformity of the polyethylene liner is good.

[0043] Step 104, cooling and demoulding to obtain a polyethylene liner.

[0044] When the polyethylene raw material is completely melted, the molding die is cooled while continuing to rotate. After it is completely cooled to room temperature, demoulding is performed, and after demoulding is completed, the molding die is cleaned, and the demoulding results in an integral rotationally molded polyethylene liner.

[0045] The cooling may be performed by forced ventilation or water spraying, as long as the temperature of the molding die is reduced to room temperature, and the specific operation method is not specifically limited.

[0046] More specifically, the step 2 is as follows: According to the winding rule, the continuous fibers of the ultra-high molecular weight polyethylene are wound on the polyethylene liner and then solidified, so that a fiber protective layer composed of ultra-high molecular weight polyethylene fibers is formed on the outer surface of the polyethylene liner.

[0047] The winding rule means that the ultra-high molecular weight polyethylene fibers should be stable and non-slip during winding, and evenly and continuously spread over the surface of the polyethylene liner, so that adjacent ultra-high molecular weight polyethylene fibers neither overlap nor separate. Through fiber winding, a fiber protective layer composed of ultra-high molecular weight polyethylene fibers with uniform and stable performance can be obtained, and the direct fiber winding method has good labor and sanitation conditions, low labor intensity, and is more conducive to cost saving.

[0048] The ultra-high molecular weight polyethylene fiber of the present invention may be wound in a circumferential manner, longitudinally or spirally, and the specific winding method is not limited as long as a tight fiber protective layer is formed on the outside of the polyethylene liner.

[0049] The circumferential winding is a winding performed along the circumferential direction of the polyethylene liner. During winding, the polyethylene liner moves at a uniform speed around its own axis, and the wire guide moves in a barrel section parallel to the axis direction of the polyethylene liner. For each rotation of the polyethylene liner, the wire guide moves a distance equal to the width of an ultra-high molecular weight polyethylene fiber. This cycle continues until the yarn is evenly distributed on the surface of the core mold cylindrical section. The circumferential winding can only be performed on the cylindrical shape of the polyethylene liner and cannot be wound onto the arc-shaped interface and valve seat. Adjacent fiber filaments are connected without overlapping, and the fiber winding angle is usually between 85° and 90°.

[0050] During the longitudinal winding, the wire guide makes uniform circular motion in a fixed plane, and the polyethylene liner rotates slowly around its own axis. Every time the wire guide rotates one circle, the polyethylene liner rotates a small angle, which is reflected on the surface of the polyethylene liner as the width of a fiber filament. The fiber filament forms an angle of 0° to 25° with the longitudinal axis of the polyethylene liner, and is tangent to the valve seats at both ends, and is continuously wound onto the polyethylene liner in sequence. The fiber filaments are arranged without fiber crossing each other, and the fiber winding trajectory is a single circular plane closed curve.

[0051] The spiral winding is also called geodesic winding. During winding, the polyethylene liner rotates at a constant speed around its own axis, and the guide wire head reciprocates along the axis direction of the polyethylene liner at a specific speed, so that spiral winding is realized on the cylinder body and the head of the polyethylene liner, and the winding angle is about 12° to 70°. In the spiral winding, the fiber winding is not only carried out on the cylindrical shape of the polyethylene liner, but also wound on the arc interface and the valve seat. The winding process of the spiral winding is as follows: the fiber filament starts from a certain point on the circumference of the valve seat, bypasses the valve seat along the curve tangent to the valve seat circle on the head surface, and bypasses the cylindrical section along the spiral trajectory, enters the valve seat at the other end, and then returns to the cylindrical section, and finally goes back to the valve seat where the winding starts, and the cycle continues until the surface of the polyethylene liner is evenly covered with fiber filaments. The characteristic of the spiral winding is that each bundle of fibers corresponds to a tangent point on the circumference of the valve seat; adjacent fiber filaments in the same direction are connected but not intersected, and fibers in different directions intersect.

[0052] More specifically, Figure 4 As shown, the step 3 is specifically as follows: Step 301: irradiate the fiber protective layer with laser to melt the ultra-high molecular weight polyethylene fiber.

[0053] By irradiating the outer surface of the fiber protective layer with laser, a laser path is formed on the fiber protective layer, and the heat generated by the laser melts the ultra-high molecular weight polyethylene fiber in the laser path area to generate a laser gap band. The ultra-high molecular weight polyethylene fiber in the laser gap band is in a molten viscous liquid state, while the ultra-high molecular weight polyethylene fiber outside the laser gap band is still in a solid state of fiber filaments.

[0054] The laser emitting the laser may be a synthetic crystal of neodymium-doped yttrium aluminum garnet (Nd 3+ :YAG), semiconductor diode, carbon dioxide (CO2) laser, etc. It is sufficient to ensure that the generated laser temperature reaches above the melting point of the ultra-high molecular weight polyethylene fiber. The melting point of the ultra-high molecular weight polyethylene fiber is approximately between 135°C and 145°C, so the laser temperature selected in this embodiment reaches 150°C.

[0055] When using a neodymium-doped yttrium aluminum garnet synthetic crystal or a semiconductor diode laser, the ultra-high molecular weight polyethylene fiber can be melted at a linear speed of more than 20 m / min. When using a carbon dioxide laser, the speed of melting the ultra-high molecular weight polyethylene fiber can be as high as 750 m / min. Therefore, the wider and longer the irradiated area, the longer the laser irradiation time. In this embodiment, there are four sizes, the largest of which is a hydrogen cylinder with a diameter of 219 mm, a height of 1680 mm, and a volume of 50 L, so the laser irradiation time should be less than or equal to 3 s.

[0056] Step 302: irradiate the polyethylene liner with laser to melt the surface of the polyethylene liner.

[0057] The laser is used to irradiate the polyethylene liner area corresponding to the laser slit band on the fiber protective layer. The heat generated by the laser melts the surface of the polyethylene liner to produce a surface melting band. The polyethylene liner at the surface melting band is in a molten viscous liquid state, while the polyethylene liner outside the surface melting band is still in a solid state.

[0058] The inner surface of the polyethylene liner, that is, the side away from the fiber protective layer, is irradiated with a laser, and the polyethylene liner is melted by laser irradiation to form a surface melting zone. The surface melting zone corresponds to the laser gap zone of the fiber protective layer, that is, the two are in the same position in the circumferential direction of the hydrogen cylinder.

[0059] The laser can be the same as or different from the laser in step 301, as long as it can reach above the melting point of the polyethylene, which is 115°C to 135°C; the same laser is used in this embodiment. Since the melting point of the polyethylene is lower than the melting point of the ultra-high molecular weight polyethylene fiber, when using laser irradiation, the irradiation time of the polyethylene liner should be less than the irradiation time of the ultra-high molecular weight polyethylene fiber. More preferably, when irradiating the polyethylene liner, the moving speed of the laser should be increased by between 10% and 50% compared with the moving speed of the laser when irradiating the ultra-high molecular weight polyethylene fiber.

[0060] Preferably, the laser can be mounted on a mobile device with a guide rail, and through the movement of the mobile device, the laser can be extended into the polyethylene liner without damaging the polyethylene liner, thereby achieving laser irradiation of the polyethylene liner and obtaining a polyethylene liner with a surface melting zone. At the same time, due to the setting of the guide rail, the alignment of the surface melting zone and the laser gap zone is more convenient and intuitive.

[0061] Step 303: Connect the fiber protective layer and the polyethylene liner by pre-tensioning to obtain a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder.

[0062] The polyethylene liner and fiber protective layer after laser irradiation are placed at room temperature for cooling and solidification. The heat-melted area after laser irradiation will be bonded due to the effect of pre-tension and then gradually cooled to room temperature to obtain a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder in which the polyethylene liner and the ultra-high molecular weight polyethylene fiber are connected as one.

[0063] The pre-tension refers to a certain tension applied to the sample in advance to straighten the sample without causing elongation. Applying appropriate pressure to the bonding area surface of the polyethylene liner and the fiber protective layer will make the molten polyethylene and ultra-high molecular weight polyethylene fibers transition from elasticity to plasticity, and can also promote the mutual diffusion of molecules and squeeze out the residual air in the weld, thereby increasing the sealing performance of the contact area between the two.

[0064] The present invention discloses a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder and a preparation method thereof. First, the polyethylene liner and the fiber protective layer of the ultra-high molecular weight polyethylene fiber are connected as one by laser curing. The method is simple, safe and easy to implement. Secondly, the ultra-high molecular weight polyethylene fiber is used, which has high strength, light weight, economical price and is convenient for mass production. Finally, the polyethylene liner and the ultra-high molecular weight polyethylene fiber are both polyethylene in nature. Therefore, the obtained hydrogen cylinder is made entirely of polyethylene material, which can be recycled, avoiding the problem of waste and being more economical.

[0065] The above content is an explanation of the preferred embodiments of the present invention, which can help those skilled in the art to more fully understand the technical solution of the present invention. However, these embodiments are merely illustrative, and it cannot be determined that the specific implementation methods of the present invention are limited to the description of these embodiments. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, several simple deductions and transformations can be made, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder, characterized in that: It includes a polyethylene liner and a fiber protective layer formed by winding ultra-high molecular weight polyethylene fibers; the polyethylene liner contains hydrogen and serves as a gas barrier; The polyethylene liner is cylindrical, and is provided with arc-shaped interfaces at both ends, wherein the arc-shaped interfaces include a seat opening connected to the valve seat and an arc-shaped surface located at the edge of the seat opening; a valve seat is provided on the outer side of the arc-shaped interface, and sealing is performed through the valve seat; The fiber protective layer serves as a load-bearing structure, surrounding the polyethylene inner liner inside, thereby protecting the polyethylene inner liner and having a certain pressure resistance.

2. A polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder according to claim 1, characterized in that: The wall thickness of the polyethylene liner is 5 mm to 20 mm; the ratio of the length to the inner diameter of the polyethylene liner is 4:1 to 5:

1.

3. The polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder according to claim 1, characterized in that: The polyethylene liner has a surface melting zone, and the fiber protective layer has a laser slit zone in the area corresponding to the surface melting zone; the surface melting zone and / or the laser slit zone are arranged along the axial direction of the polyethylene liner and / or the fiber protective layer, and are equal to the length of the polyethylene liner and the fiber protective layer; The surface melting zone and the laser slit zone are adhered to connect the polyethylene liner and the fiber protective layer into a whole.

4. A method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder, used to prepare the polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder, characterized in that: The following steps are involved: Step 1, obtaining a polyethylene liner by rotational molding; Step 2, winding ultra-high molecular weight polyethylene fiber on the outside of the polyethylene liner to form a fiber protective layer; Step 3: Laser irradiates the fiber protective layer and the polyethylene liner to melt the two, and connect them into one through pre-tension.

5. The method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder according to claim 4, characterized in that: The step 1 specifically includes: Step 101, applying a release agent on each component of the molding die, and assembling the coated molding die components to obtain a molding die; Step 102, adding polyethylene raw material into the molding die and installing it on a rotating machine; Step 103, heating the molding die and rotating it around a rotation axis; Step 104, cooling and demoulding to obtain a polyethylene liner.

6. The method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder according to claim 5, characterized in that: The rotating machine has a rotatable main shaft fixed arm and an adjusting disk as a secondary shaft, the molding die is placed horizontally with the rotation center and the swing center in the horizontal direction, and the center of the inner liner coincides with the rotation center and the swing center; The rotation speed of the fixed arm is called the arm speed, the rotation speed of the adjustment disk is called the disk speed, and the arm speed is divided by the difference between the disk speed and the arm speed as the speed ratio; The product is manufactured under the condition that the speed ratio range is less than 1:2, and then annealed and cooled to obtain an inner container with a flat inner surface.

7. The method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder according to claim 6, characterized in that: The rotation speed of the molding die around the axis is 1 r / min, the swing angle is ±45°, the extreme position dwell time is 0 s, and the swing speed is 6.5 times / min. At this time, the wall thickness tolerance of the polyethylene liner is controlled at 5.89 mm ± 0.53 mm.

8. The method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder according to claim 4, characterized in that: The step 3 is specifically as follows: Step 301, irradiating the fiber protective layer with a laser to melt the ultra-high molecular weight polyethylene fiber; Step 302, irradiating the polyethylene liner with a laser to melt the surface of the polyethylene liner; Step 303: Connect the fiber protective layer and the polyethylene liner by pre-tensioning to obtain a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder.

9. The method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder according to claim 8, characterized in that: By laser irradiation, a laser path is formed on the fiber protective layer, and the heat generated by the laser melts the ultra-high molecular weight polyethylene fiber in the laser path area to generate a laser gap band; The laser temperature reaches 150° C.; and the laser irradiation time is less than or equal to 3 seconds.

10. The method for preparing a polyethylene-ultra-high molecular weight polyethylene fiber hydrogen cylinder according to claim 8, characterized in that: Using laser to irradiate the polyethylene liner area corresponding to the laser slit band on the fiber protective layer, the heat generated by the laser melts the surface of the polyethylene liner to produce a surface melting band; The moving speed of the laser irradiating the polyethylene liner should be increased by 10% to 50% compared with the moving speed of the laser irradiating the ultra-high molecular weight polyethylene fiber.

Citation Information

Patent Citations

  • Composite gas cylinder and forming method thereof

    CN111779965A

  • Hydrogen storage cylinder for explosion-proof hydrogen fuel cell automobile and manufacturing method thereof

    CN114033962A

  • Nonmetal composite pipe for conveying hydrogen and manufacturing method

    CN115773407A

  • Rotational molding process for plastic inner container of IV-type hydrogen storage cylinder

    CN116922648A

  • Hydrogen storage cylinder plastic inner container of composite structure and rotational molding process of hydrogen storage cylinder plastic inner container

    CN117087061A