Anti-fatigue flexible strain sensor based on multi-scale stress dispersion mechanism

By adopting a multi-scale stress dispersion mechanism and polymer network structure in flexible strain sensors, combining the design of low-conductive and high-conductive layers, embedded hard elastomer fibers and using polypyrrole/graphene oxide composites, the flexible strain sensor is solved. Fatigue damage and conductive layer stability issues achieve high sensitivity and wide operating range sensors.

CN119022775AActive Publication Date: 2024-11-26HEFEI UNIV OF TECH +1

Patent Information

Application Number
CN202411121272.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Existing flexible strain sensors are prone to permanent fatigue damage under alternating loads, resulting in poor stability, limited sensitivity and working range, and the conductive layer is prone to failure.

Method used

Using a multi-scale stress dispersion mechanism, a polymer network formed by polyethyl acrylate and 3-(trimethoxysilyl)propylene methacrylate functionalized silica nanoparticles combines low-conductive and high-conductive layers. Structural design, embedded hard elastomer fibers into the inner core of the soft elastomer, and improved conductivity and dispersion using polypyrrole/graphene oxide composites.

Benefits of technology

The fatigue threshold and stability of the sensor are significantly improved, high sensitivity and wide working range are achieved, while avoiding the shedding of the conductive layer and electrical failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119022775A_ABST
    Figure CN119022775A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-fatigue flexible strain sensor based on a multi-scale stress dispersion mechanism. The anti-fatigue flexible strain sensor structurally comprises a low-conductivity inner core, a high-conductivity layer and a packaging layer which are sequentially sleeved from inside to outside, the low-conductivity inner core comprises a flexible base body of a cylindrical structure. Grooves are evenly distributed in the surface of the flexible base body in the circumferential direction, the grooves are through in the axial direction of the flexible base body, and the cross sections of the grooves are rectangular. Each groove of the flexible substrate is filled with a low-conductivity material; the high-conductivity layer is cylindrical and covers the surface of the low-conductivity inner core; a plurality of annular bulge structures are uniformly distributed on the surface of the high-conductivity layer along the axial direction; and the packaging layer coats the surface of the high-conductivity layer, so that the whole flexible strain sensor is of a cylindrical strip structure. The prepared flexible strain sensor has the characteristics of fatigue resistance, wide sensing range, high sensitivity and stability and the like, can be used in the field of human body wearable and the field of robot skin, and has good practicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of sensors, and in particular relates to an anti-fatigue flexible strain sensor based on a multi-scale stress dispersion mechanism and a preparation method thereof. Background Art

[0002] Flexible strain sensors, with their excellent advantages of lightness, flexibility, portability, stretchability and low cost, have become the research focus in the fields of wearable devices and robot skin. Flexible strain sensors based on crack structures have attracted much attention due to their simple preparation, high sensitivity and fast response. However, the narrow sensing range, disordered crack structure and deformation and fracture of the substrate due to fatigue cause changes in the crack structure and failure, which greatly limits the practical application and service life of such sensors.

[0003] In recent years, people have done a lot of work on the research of flexible strain sensors against fatigue and stability:

[0004] The academic paper "An anti-fatigue design strategy for 3D ribbon-shaped flexible electronics (Cheng X, Zhang F, Bo R, et al. An anti-fatigue design strategy for 3D ribbon-shaped flexible electronics. Adv Mater. 2021; 33 (37): 2102684.) proposed converting metal-dominated failure to the desired polymer-dominated failure, by adding an ultra-thin polymer layer (such as polyimide, PI) on top of the metal layer (such as copper, copper), significantly extending the fatigue life of 3D ribbon-shaped flexible electronic devices. The demonstrated 3D resistive sensor can be used in 10 5 Long-term vibration measurements during 10 loading cycles.

[0005] Academic paper "Tough and anti-fatigue double network gelatin / polyacrylamide / DMSO / Na 2 SO 4Ionic conductive organohydrogel for flexible strain sensor"(Jing Lu,Oudong Hu,Jianfeng Gu,Guoqi Chen,Dezhan Ye,Linxi Hou,Xi Zhang,Xiancai Jiang,Tough and anti-fatigue double network gelatin / polyacrylamide / DMSO / Na 2 SO 4 A hybrid double network organohydrogel with physical and chemical crosslinking was proposed in this paper. The gelatin / PAM / DMSO / Na2O3 was prepared by forming a physical crosslinking network with gelatin through sol-gel transition and salting-out effect, and a chemical crosslinking network with polyacrylamide (PAM) chains. 2 SO 4 The organic hydrogel showed high fatigue resistance in 1,000 stretching cycles at a fixed strain of 300%, without obvious plastic deformation. The hydrogel was assembled into a multifunctional sensor with high sensitivity, accuracy and stability. However, since the hydrogel easily loses water and becomes dry during use, the sensor has a short service life.

[0006] The academic paper "A wave-inspired ultrastretchable strain sensor with predictable cracks" (Qiang Zou, Jia Zheng, Qi Su, WanLi Wang, Wei Gao, Zhuomin Ma, A wave-inspired ultrastretchable strain sensor with predictable cracks, Sensors and Actuators A: Physical, Volume 300, 2019, 111658, ISSN 0924-4247,) proposed a flexible strain sensor based on GO / PDMS with a wave structure. Through the wavy microstructure, the stress is better concentrated in the groove, the stress from both sides to the middle of the groove is reduced, and the generation of disordered cracks is avoided. However, the sensitivity of the sensor is low (GF≈80) under 0-30% strain, and because the stress sensitive element uses a single graphene material, this material is easy to aggregate.

[0007] Patent CN115993086B proposes a method for mechanical modification of flexible sensors based on PEDOT:PSS. By adding polyvinyl alcohol, formaldehyde and glycerol to PEDOT:PSS, the acetal reaction between polyvinyl alcohol and formaldehyde is used to produce a polyvinyl alcohol cross-linked network, and a large number of hydroxyl groups of glycerol are connected with polyvinyl alcohol polymer chains through hydrogen bonds to strengthen the polyvinyl alcohol cross-linked network. The cross-linked network and PEDOT:PSS form an interpenetrating network, which greatly enhances the mechanical properties of the mixed network. When used in wearable devices, good air permeability is required, but PEDOT:PSS is easy to absorb moisture and has poor wettability. It will absorb human sweat and moisture in the air and decompose and fail.

[0008] Patent CN115678132B proposes a method for preparing anti-fatigue rubber. The invention introduces multi-dimensional nanofillers into the rubber base material, namely spherical carbon black, tubular nanofiller carbon nanotubes, and flaky nanofiller graphene oxide. The filler network structure formed by these fillers in the rubber matrix is ​​strong, which limits the mobility of the rubber molecular chain and causes the crack tip morphology to evolve continuously during expansion, resulting in new morphologies such as passivation, deflection, and branching, thereby reducing the crack propagation rate.

[0009] Patent CN110823085B proposes a flexible strain sensor with a regular crack structure and its manufacturing method, which solves the problems of poor consistency, poor reliability and low repeatability of existing flexible strain sensors based on the method of cutting after printing or direct printing. However, the sensor does not solve the problem of crack propagation during repeated use, and the location and number of cracks cannot be adjusted.

[0010] In summary, although some progress has been made in the research of stability and consistency of flexible strain sensors, there are still the following shortcomings:

[0011] 1. Under the action of alternating loads, the supporting material of the flexible strain sensor undergoes local deformation in the high stress area. This repeated deformation will cause the bond strength between atoms or molecules to be destroyed, causing the atoms or molecules of the material to move and rearrange, resulting in permanent fatigue damage to the sensor. This fatigue damage will cause irreversible plastic deformation of the supporting material, and the conductive layer attached to the supporting material will change accordingly. The sensor characteristics will continue to change with time and stress, and the sensor stability will be poor.

[0012] 2. During the repeated loading and unloading process, fatigue damage of the flexible strain sensor continues to develop at the microscopic level to form macroscopic fine cracks. The sensor may also create cracks when it hits sharp objects during use. The crack tip will rapidly expand in each loading cycle due to stress concentration. When the crack rapidly expands to a sufficient length and reaches a critical size, the sensor will physically break or electrically fail, thus affecting the use of the sensor.

[0013] 3. In order to improve the sensitivity of the flexible strain sensor, a crack-type surface microstructure is introduced into the stress-sensitive element of the sensor, but the flexible strain sensor based on the single-layer crack structure cannot have both high sensitivity and wide working range. When the stress-sensitive element forms a transversely cut channel crack, it has ultra-high sensitivity, but the conductive path is quickly cut off under small deformation, and the stretchability is usually less than 5%; when the stress-sensitive element forms a network crack with random distribution in direction and short length, the stretchability is usually higher than 40%, but due to the increase in the number of conductive paths and the decrease in crack propagation efficiency under deformation, the sensitivity is low.

[0014] 4. Based on the flexible strain sensor of crack structure, stress sensitive elements are mostly made by adding carbon conductive materials into polymers, but the conductive fillers are not evenly dispersed in the polymers, resulting in poor stability of the sensor. Another method is to use conductive polymers to prepare stress sensitive units, but conductive polymers have poor stretchability and low intrinsic conductivity, which cannot meet the sensor requirements.

[0015] 5. When the strain sensor based on crack structure is cyclically stretched, the stress slowly decreases from both sides to the middle. Since the uniform stress in a large area may cause the generation and connection of random cracks at the same time, the position, number and distribution of cracks generated in the stress sensitive element are random, and the stability and consistency of the sensor are poor.

[0016] 6. The stress-sensitive element of the crack strain-based sensor is generally a planar membrane structure. The cracks caused by this structure can only be confined to the two-dimensional (2D) surface, which limits the further improvement of the sensor sensitivity. Secondly, due to the difference in mechanical properties and surface properties, debonding or delamination is prone to occur between the elastomer and the conductive layer with a flat membrane structure, which may reduce the mechanical robustness of the sensor. Summary of the invention

[0017] In order to solve the above technical problems, the present invention provides an anti-fatigue flexible strain sensor based on a multi-scale stress dispersion mechanism and a preparation method. On the one hand, the fatigue threshold is amplified by the synergistic effect of long polymers, clustered particles and strong polymer-particle adhesion in the polymer network formed by silica nanoparticles functionalized with polyethyl acrylate (PEA) and 3-(trimethoxysilyl) propyl methacrylate (TPM). And the polymer network is electrically modified to prepare a film with good anti-fatigue performance and controllable electrical properties. On the other hand, the modulus of the polymer is controlled by regulating the content of TPM-functionalized silica nanoparticles in PEA, and the polymer fiber with a high elastic modulus is embedded in the inner core matrix with a low elastic modulus. The fiber and the inner core matrix are adhered together by covalent interconnection, and the fatigue threshold is further amplified. The anti-fatigue flexible strain sensor prepared by the present invention can be widely used in the fields of wearable devices and electronic skin.

[0018] In order to solve the above problems, the present invention adopts the following technical solutions:

[0019] The present invention firstly discloses an anti-fatigue flexible strain sensor based on a multi-scale stress dispersion mechanism. The strain sensor comprises a low-conductivity inner core, a high-conductivity layer and a packaging layer which are sequentially arranged from the inside to the outside.

[0020] The low-conductivity inner core comprises a flexible substrate with a cylindrical structure; the surface of the flexible substrate is uniformly provided with grooves along the circumferential direction, the grooves penetrate the flexible substrate along the axial direction and have a rectangular cross-section; each groove of the flexible substrate is filled with a low-conductivity material, and the low-conductivity material matches the shape of the groove; the low-conductivity inner core is formed by a flexible substrate equipped with a low-conductivity material.

[0021] The high-conductivity layer is cylindrical and covers the surface of the low-conductivity inner core; the surface of the high-conductivity layer is evenly distributed with a number of annular protrusion structures along the axial direction;

[0022] The packaging layer is coated on the surface of the high conductive layer, so that the flexible strain sensor has a cylindrical long strip structure as a whole.

[0023] Furthermore, the flexible substrate and the encapsulation layer are prepared from silicon dioxide nanoparticles functionalized with polyethyl acrylate and 3-(trimethoxysilyl)propyl methacrylate.

[0024] Furthermore, the diameter of the flexible substrate is 500 μm to 1 mm, and the stretchable length is not less than 200%; the number of grooves uniformly distributed along the circumference of the flexible substrate is 5 to 10.

[0025] Further, the low-conductive material is made of polyethyl acrylate, 3-(trimethoxysilyl)propyl methacrylate functionalized silica nanoparticles and polypyrrole. The electrical conductivity of the low-conductive material is not higher than 10S / cm, and the stretchable length is not lower than 200%. The electrical conductivity of the low-conductive material can be adjusted by adjusting the amount of polypyrrole within a limited range according to demand, and the elastic modulus of the low-conductive material can be adjusted by adjusting the amount of TPM functionalized silica nanoparticles within a limited range according to demand, and the elastic modulus of the low-conductive material is higher than the elastic modulus of the flexible substrate.

[0026] Further, the high conductive layer is prepared from polypyrrole, graphene oxide and phytic acid. The conductivity of the high conductive layer is not less than 4000S / cm, and the elongation at break is not more than 2%. Polypyrrole is one of the most important conductive polymers, with the advantages of easy synthesis, good stability, low price and high conductivity. However, polypyrrole usually causes serious aggregation due to intermolecular interactions, and has the defects of poor dispersibility and processability. One method to overcome these shortcomings is to deposit PPy on a carbon-based material. Since graphene oxide has the characteristics of high specific surface area, chemical stability, high π conjugation and hydrophilicity, it can provide an excellent electrode platform for adsorbing other molecules. PPy with π bonds on the pyrrole ring can be adsorbed on the surface of graphene oxide through π-π stacking interactions, hydrogen bonds and van der Waals interactions. Nanocomposites based on polypyrrole and graphene oxide show synergistic properties, which enhance the conductivity and dispersibility of conductive polymers. The conductivity of the high conductive layer can be adjusted according to demand by adjusting the amount of pyrrole, graphene oxide and phytic acid within a limited range.

[0027] Furthermore, each annular protrusion structure on the surface of the highly conductive layer has a width of 400-800 μm and a protrusion height of 100-400 μm, and an annular crack extending circumferentially of the highly conductive layer is formed at the junction of each annular protrusion structure and the surface of the highly conductive layer by pre-stretching.

[0028] The conductivity of the low conductive material is not higher than 10S / cm, and the conductivity of the high conductive layer is not lower than 4000S / cm. The sensitivity of the sensor is defined as the ratio of the change in sensor resistance to the initial resistance after a unit tensile strain is generated. The conductivity of the inner and outer conductive layers is different, and the sensing performance of the entire sensor device is also different. The high conductivity of the outer layer makes the initial resistance of the sensor small enough, and the low conductivity of the inner core prevents the sensor from electrical failure under large stretching, so that the sensor has the characteristics of a wide sensing range. The sensitivity of the sensor prepared according to the above-mentioned inner and outer layer conductivity reaches more than 2000.

[0029] The elongation at break of the low-conductivity material is not less than 200%, and the elongation at break of the high-conductivity layer is not more than 2%. When the elongations at break of the inner and outer layers are different, under the stretched state, since the mechanical properties of the inner core are better than those of the outer layer, under the stretched state, the deformation of the high-conductivity outer layer of the sensor will reach the elongation at break first and cause cracks.

[0030] Fatigue fracture is a brittle fracture in the macroscopic sense, because the sample is subjected to elastic deformation as a whole; however, in the microscopic sense, once a crack is generated, there will be a plastic deformation zone at the front of the crack in the initial stage of expansion. The fatigue threshold is usually used to describe the material's resistance to fatigue damage. A higher fatigue threshold means that the material will begin to suffer fatigue damage only at a higher number of cycles or a larger stress amplitude.

[0031] The low-conductivity inner core is cylindrical, and the high-conductivity layer is coated on the outside of the cylinder. Preferably, the diameter of the cylinder is 500μm to 1mm. The low-conductivity inner core is formed by embedding hard elastomer fibers (i.e., low-conductivity materials) into a soft elastomer matrix. Preferably, grooves for assembling low-conductivity materials are provided on the surface of the flexible matrix at 36° to 72° intervals along the circumference, and the width accounts for 2% to 5% of the circumference of the bottom surface of the cylinder. In the generalized Lake-Thomas model, cracks extend by breaking hard fibers, and the threshold is equal to the elastic energy stored in a layer of fiber per unit area. At the front end of the crack in the composite material, the soft matrix is ​​sheared violently, causing the stress to be dispersed in the hard lattice. The large shearing action of the soft matrix will relieve the crack front, the stress of the hard fiber is concentrated, and the crack is first blocked by the hard fiber. Once the crack cuts the fiber, a large amount of elastic energy stored in the fiber will be released, greatly improving the fatigue threshold of the low-conductivity layer.

[0032] Core composites rely on a multi-scale stress dispersion mechanism to improve the fatigue threshold of materials. First, through the covalent interconnection between particles and polymers, the strong adhesion between polymers and particles through covalent bonds allows high stresses to be transferred from polymers to particles. In this way, stress can be dispersed in many interparticle gaps in the particle cluster, and when one gap ruptures, the energy stored in multiple gaps will be dissipated. Second, the presence of long polymer chains in the composite helps stress dispersion. When a crack hits a particle cluster, the rigid particles disperse the stress into multiple gaps in the particle cluster. The rupture of a single gap releases the energy stored in multiple gaps, resulting in stress dispersion at the polymer and particle scales. Finally, the aggregation of particles further enhances stress dispersion. Even without particle percolation, clustered particles can disperse stress into multiple polymer thin layers between clustered particles. This multi-scale stress dispersion improves the fatigue threshold of the composite.

[0033] The method for preparing the fatigue-resistant flexible strain sensor based on the multi-scale stress dispersion mechanism of the present invention comprises the following steps:

[0034] Step 1: Prepare flexible substrate and encapsulation layer slurry

[0035] The silica nanoparticles functionalized with 3-(trimethoxysilyl)propyl methacrylate and the monomer ethyl acrylate are uniformly mixed in N,N-dimethylformamide, tricyclo[5.2.1.02,6]decanedioic acid diacrylate as a crosslinking agent and 2-hydroxy-2-methylpropiophenone as a photoinitiator are added, and the mixture is stirred at room temperature to obtain a flexible matrix and an encapsulation layer slurry; wherein the ratio of the mass of the nanoparticles to the volume of ethyl acrylate is 0.4-0.6 g:1 mL, and the molar ratio of the crosslinking agent to the monomer is 10 -4 ~10 -3 : 1, the molar ratio of the photoinitiator to the crosslinking agent is 0.3-0.4:1;

[0036] Step 2: Prepare low conductive material slurry

[0037] 3-(trimethoxysilyl) propyl methacrylate functionalized silica nanoparticles and monomer ethyl acrylate are mixed evenly in N,N-dimethylformamide, tricyclo[5.2.1.02,6]decanedioic acid diacrylate as a crosslinking agent and 2-hydroxy-2-methylpropiophenone as a photoinitiator are added, stirred at room temperature for reaction, and then polypyrrole is added and ultrasonically mixed evenly to obtain a low conductive material slurry; wherein: the ratio of the mass of the nanoparticles to the volume of ethyl acrylate is 0.7-0.9 g: 1 mL; the molar ratio of the crosslinking agent to the monomer is 10 -4 ~10 -3: 1, the molar ratio of the photoinitiator to the crosslinking agent is 0.3-0.4:1; the mass ratio of the nanoparticles to the polypyrrole is 1600-1700:1;

[0038] Step 3: Prepare high conductive layer slurry

[0039] Graphene oxide nanosheets were dispersed in water, pyrrole was added and mixed evenly, and FeCl 3 -6H 2 O, stirring polymerization reaction was carried out at 0-4°C, and the obtained product was filtered, washed and vacuum dried to obtain polypyrrole / graphene oxide nanocomposite material; wherein graphene oxide nanosheets, FeCl 3 -6H 2 O. The dosage ratio of pyrrole is 15-20 mg: 0.3-0.4 g: 30 μL;

[0040] Ultrasonic dispersion of polypyrrole / graphene oxide nanocomposite in phytic acid solution to obtain high conductive layer slurry; wherein the amount ratio of polypyrrole / graphene oxide nanocomposite to phytic acid is 100-110 g:1 mol;

[0041] Step 4: Prepare the sensor by using a casting process combined with mold forming

[0042] The flexible substrate and the encapsulation layer slurry are poured into the substrate mold and UV-cured to form a flexible substrate with grooves uniformly distributed on the surface along the circumferential direction; the low-conductive material slurry is then injected into the grooves of the flexible substrate and UV-cured to form a low-conductive inner core; the low-conductive inner core is repeatedly stretched 2000-3000 times under a strain of 15-30% to stabilize the microstructure of the inner core;

[0043] The low-conductivity inner core is straightened and suspended and positioned at the central axis of the high-conductivity mold, the high-conductivity layer slurry is cast into the high-conductivity layer mold to wrap the inner core, and then the bubbles are removed by vacuum, infrared curing and drying are carried out; the device is taken out and repeatedly stretched 10 to 50 times at a strain of 15 to 30%, so that the high-conductivity layer forms regular annular cracks extending along the circumference of the high-conductivity layer at the junction of each annular protrusion structure and the surface of the high-conductivity layer; two wires are fixed at both ends of the axial direction of the high-conductivity layer;

[0044] The prepared device is straightened and suspended in the center of a cylindrical packaging layer mold, and then the flexible substrate and packaging layer slurry are poured into the packaging layer mold and UV-cured to obtain a fatigue-resistant flexible strain sensor based on a multi-scale stress dispersion mechanism.

[0045] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0046] 1. The flexible strain sensor proposed in the present invention has a high fatigue threshold and good stability. Its inner core has an extremely high fatigue threshold of more than 1000Jm -2 . The inner core uses ethyl acrylate as a monomer to synthesize the polymer. Since the polymer chain is very long, the number of entanglements greatly exceeds the number of crosslinks. The dense entanglements enable the tension to be transmitted to many other chains along the length of the polymer chain. The sparse crosslinks prevent the polymer chains from separating, making the polymer have high toughness and fatigue resistance. By adding TPM-functionalized nano-silica particles to polyethyl acrylate, the polymer chains and particles are interconnected by strong bonds. When a crack hits a cluster of particles, the rupture of a single particle-particle gap dissipates the energy stored in many particle-particle gaps in the cluster, further increasing the fatigue threshold of the polymer. At the same time, it limits the movement of the polymer chain and inhibits the permanent plastic deformation of the polymer.

[0047] 2. The flexible strain sensor proposed in the present invention has an inner core with two alternating moduli. By embedding hard elastomer fibers into a soft elastomer inner core matrix, the crack propagation rate is greatly hindered. When the inner core produces small cracks due to periodic loading and unloading, the large shearing action of the soft matrix disperses the stress at the front end of the crack. Further crack propagation requires breaking of the hard fibers. The crack needs to break through the elastic energy stored in the hard fibers, which hinders the crack propagation and achieves high toughness and low hysteresis.

[0048] 3. The flexible strain sensor proposed in the present invention uses a low-conductivity fiber embedded in a matrix and a high-conductivity outer layer to bond together to form a strain sensitive element of the flexible strain sensor, so that the flexible strain sensor has high sensitivity and a wide working strain range.

[0049] 4. The flexible strain sensor proposed by the present invention has a high-conductivity layer conductive material made of polypyrrole / graphene oxide / phytic acid. The mixed conductive material exhibits superior performance by integrating the advantages of the components. Due to the strong π-π interaction and van der Waals force, pyrrole can be adsorbed on the surface of graphene oxide, grow and combine with graphene oxide, making it easier for carriers to move, thereby increasing conductivity. It can also effectively improve the uniformity of graphene oxide and pyrrole, inhibit the high inter-sheet junction contact resistance of graphene and the aggregation of pyrrole. The addition of phytic acid can increase additional carriers, and the anions in phytic acid can move in polypyrrole to form ion conduction channels, promote ion conduction in polypyrrole, and further enhance conductivity.

[0050] 5. The flexible strain sensor proposed in the present invention adopts a stress concentration strategy for the high conductive layer, so that the stress of the sensor is concentrated under the pre-stretching strain, avoiding the random generation of cracks in the sensor, thereby obtaining high consistency of the sensor during the manufacturing process and high stability during use.

[0051] 6. The flexible strain sensor proposed in the present invention has various sensitivity adjustment methods. The sensitivity can be flexibly adjusted by changing the number, width and depth of the substrate grooves, and the sensitivity of the sensor can be flexibly adjusted by changing the conductivity of the low-conductive material of the inner core and the high-conductive outer layer.

[0052] 7. The flexible strain sensor proposed in the present invention adopts a linear structure to expand the crack into a three-dimensional structure, so that the sensor has higher sensitivity and is easier to sew with the fabric; at the same time, the outermost layer is encapsulated with a PEA and TPM functionalized silica composite material, which effectively inhibits the shedding of the high-conductivity layer, protects the film and provides hydrophobicity.

[0053] 8. The materials used in the flexible strain sensor proposed in the present invention, such as ethyl acrylate, pyrrole, TPM-functionalized silica, phytic acid, etc., are non-toxic and biocompatible, and can be safely used in the wearable field without causing harm to the human body. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 This is a schematic diagram of the appearance structure of the anti-fatigue flexible strain sensor based on the multi-scale stress dispersion mechanism of the present invention;

[0055] Figure 2 It is a schematic diagram of a low-conductivity inner core and a high-conductivity layer of an anti-fatigue flexible strain sensor based on a multi-scale stress dispersion mechanism of the present invention;

[0056] Figure 3 It is a schematic diagram of the cross-sectional structure of the fatigue-resistant flexible strain sensor based on the multi-scale stress dispersion mechanism of the present invention;

[0057] Figure 4 A schematic diagram of a mold used in manufacturing a flexible substrate of a flexible strain sensor according to the present invention;

[0058] Figure 5 A schematic diagram of a mold used in manufacturing a high conductive layer of a flexible strain sensor according to the present invention;

[0059] Figure 6 It is a schematic diagram of the principle that the fatigue threshold is amplified by the synergistic effect between the long polymer single chain and clustered particles of the low-conductive inner core matrix material in the flexible strain sensor of the present invention;

[0060] Figure 7 The schematic diagram of the flexible strain sensor of the present invention is that the low conductive core prevents crack propagation by embedding hard fibers into the soft matrix;

[0061] Figure 8 The schematic diagram of the present invention for preventing the coagulation of polypyrrole / graphene composite conductive materials;

[0062] Fig. 9A schematic diagram of tensile stress distribution of a high-conductive layer bionic structure of an anti-fatigue flexible strain sensor based on multi-scale stress according to the present invention;

[0063] Fig.10 A schematic diagram of the sensing mechanism and local conductive path of the anti-fatigue flexible strain sensor based on the multi-scale stress dispersion mechanism of the present invention;

[0064] Fig.11 The stress-strain characteristic curve of the fatigue-resistant flexible strain sensor based on the multi-scale stress dispersion mechanism of the present invention;

[0065] Fig.12 The strain-resistance characteristic curve of the anti-fatigue flexible strain sensor based on the multi-scale stress dispersion mechanism of the present invention;

[0066] Fig.13 The cyclic stretching-resistance characteristic curve of the fatigue-resistant flexible strain sensor based on the multi-scale stress dispersion mechanism under different strains of the present invention;

[0067] Fig.14 It is the step strain-resistance characteristic curve of the anti-fatigue flexible strain sensor based on the multi-scale stress dispersion mechanism of the present invention;

[0068] Fig.15 This is the electrical stability curve of the fatigue-resistant flexible strain sensor based on the multi-scale stress dispersion mechanism of the present invention. DETAILED DESCRIPTION

[0069] The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.

[0070] The ethyl acrylate used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (AR 99%).

[0071] Tricyclo[5.2.1.02,6]decanedioic acid diacrylate used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0072] The 2-hydroxy-2-methylpropiophenone used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0073] The N,N-dimethylformamide used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (AR 99.8%).

[0074] The xylene used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (AR 99%).

[0075] The silicon dioxide particles used in the following examples were purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (average particle size 110 nm, purity > 99.5%).

[0076] 3-(Trimethoxysilyl)propyl methacrylate used in the following examples was purchased from Sigma-Aldrich (AR 98%).

[0077] The pyrrole used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (AR 98%).

[0078] The polypyrrole used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0079] The graphene oxide used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (sheet diameter: 0.5-5 μm, thickness: 0.8-1.2 nm).

[0080] The phytic acid used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (AR 50%).

[0081] The ferric chloride hexahydrate used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (purity 99%).

[0082] Example 1

[0083] like Figure 1 to Figure 3 As shown, the fatigue-resistant flexible strain sensor based on the multi-scale stress dispersion mechanism provided in this embodiment is an overall cylindrical strip structure (or a linear structure with a circular cross-section), including a low-conductivity inner core, a high-conductivity layer and a packaging layer which are sequentially arranged from the inside to the outside;

[0084] The low-conductivity inner core includes a flexible substrate with a cylindrical structure; the surface of the flexible substrate is evenly distributed with grooves along the circumferential direction, the grooves penetrate the flexible substrate along the axial direction, and the cross-section is rectangular; each groove of the flexible substrate is filled with a low-conductivity material, and the low-conductivity material matches the shape of the groove; the low-conductivity inner core is composed of a flexible substrate equipped with a low-conductivity material.

[0085] The high-conductivity layer is cylindrical and covers the surface of the low-conductivity inner core; the surface of the high-conductivity layer is evenly distributed with a number of annular protrusion structures along the axial direction;

[0086] The encapsulation layer is coated on the surface of the high conductive layer.

[0087] The method for preparing the anti-fatigue flexible strain sensor of this embodiment comprises the following steps:

[0088] Step 1: Prepare flexible substrate and encapsulation layer slurry

[0089] Preparation of TPM-functionalized silica nanoparticles: 30 g of dried silica nanoparticles were stirred into a suspension in 600 mL of xylene, 180 mL of xylene solution and 50 mL of 3-(trimethoxysilyl)propyl methacrylate solution were added within 25 minutes, and refluxed at 140 °C under nitrogen for 8 hours. After cooling to room temperature, the suspension was filtered and washed with toluene, and dried in vacuum at 100 °C for 6 hours. The obtained TPM-functionalized silica nanoparticles were 2 O 5 Store in a desiccator.

[0090] In a fume hood: 6.2 g of TPM functionalized silica nanoparticles were weighed and poured into a conical tube. Then 10.8 mL of ethyl acrylate with a density of 0.918 g / mL and 30 mL of N,N-dimethylformamide solution were added to the conical tube. The mixture was stirred at 3000 rpm for 1 minute in a vortex mixer and sonicated at room temperature for 3 minutes. Then 0.024 mL of tricyclo[5.2.1.02,6]decanedioic acid diacrylate with a density of 1.1 g / mL and 0.0053 g of 2-hydroxy-2-methylpropiophenone were added and stirred again at 3000 rpm for 1 minute to obtain a flexible substrate and encapsulation layer slurry.

[0091] Step 2: Prepare low conductive material slurry

[0092] In a fume hood: 8.3 g of TPM functionalized silica nanoparticles were weighed and poured into a conical tube. Then 10.8 mL of ethyl acrylate with a density of 0.918 g / mL and 30 mL of N,N-dimethylformamide solution were added to the conical tube. The mixture was stirred at 3000 rpm for 1 minute in a vortex mixer and sonicated at room temperature for 3 minutes. Then 0.024 mL of tricyclo[5.2.1.02,6]decanedioic acid diacrylate with a density of 1.1 g / mL and 0.0053 g of 2-hydroxy-2-methylpropiophenone were added and stirred at 3000 rpm again for 1 minute. Subsequently, 5 mg of polypyrrole was added and sonicated at room temperature for 10 minutes to obtain a low conductive material slurry.

[0093] Step 3: Prepare high conductive layer slurry

[0094] 20 mg of graphene oxide nanosheets were dispersed in 40 mL of water to obtain a yellow-brown dispersion with a concentration of 0.5 mg / mL. 30 μL of pyrrole was added to the graphene oxide solution and magnetically stirred for more than 1 h. Subsequently, 20 mL of 0.32 g of FeCl 3 -6H 2 O aqueous solution, stirred at 0-4 ° C for 4 h, the obtained product was filtered, washed with ethanol and deionized water in turn, and then vacuum dried at 45 ° C for 12 h to obtain a polypyrrole / graphene oxide nanocomposite material

[0095] 10 mg of polypyrrole / graphene oxide nanocomposite material was dispersed in 10 mL of 0.01 mol / L phytic acid aqueous solution and ultrasonically treated for 2 h to form a stable polypyrrole / graphene oxide nanocomposite material suspension to obtain a high conductive layer slurry.

[0096] Step 4: Prepare the sensor by using a casting process combined with mold forming

[0097] Use silicone release agent to spray on the base glass mold (its structure is as follows Figure 4 The flexible substrate and encapsulation layer slurry were poured into the glass mold and the strength was 1.5 mW cm -2 The sample was cured by irradiating with an ultraviolet lamp for 12 hours, and then taken out from the substrate mold and placed in a fume hood for 1 day to evaporate the unreacted monomer and DMF, thereby forming a flexible substrate with grooves uniformly distributed on the surface along the circumference.

[0098] The low-conductive material slurry was injected into the grooves of the flexible substrate and again heated with an intensity of 1.5 mW cm -2 The sample was placed in a fume hood for 1 day to obtain a low-conductivity inner core. The inner core was repeatedly stretched 2000 times at 30% strain to stabilize the inner core microstructure.

[0099] The low-conductivity inner core is straightened and suspended and positioned on the high-conductivity layer mold (its structure is as follows Figure 5 The high conductive layer slurry was cast into the high conductive layer mold to wrap the linear core, and then the mold was placed in a vacuum pump with a vacuum degree of 200Pa and allowed to stand for 30 minutes to remove bubbles. -2 . irradiated with infrared light for 6 hours, and finally placed in a 60℃ oven for 4 hours; the device was taken out and repeatedly stretched 20 times at 20% strain, so that the high conductive layer formed regular annular cracks extending along the circumference of the high conductive layer at the junction of each annular protrusion structure and the surface of the high conductive layer. Two wires were fixed at both ends of the axial direction of the high conductive layer.

[0100] The silicone release agent was sprayed on the cylindrical encapsulation layer glass mold again. The prepared device was straightened and suspended in the center of the encapsulation layer mold. Then, the flexible substrate and encapsulation layer slurry were poured into the encapsulation layer mold. -2 The sample was irradiated with an ultraviolet lamp for 12 hours to solidify it, and the sample was taken out of the mold and placed in a fume hood for 1 day to obtain an anti-fatigue flexible strain sensor based on a multi-scale stress dispersion mechanism.

[0101] Specifically, in this embodiment: the diameter of the flexible substrate is 1 mm, the stretchable length is 230%, the number of grooves uniformly distributed along the circumference of the flexible substrate is 8, and the groove width accounts for 4% of the circumference of the cylindrical bottom surface of the substrate. The conductivity of the low-conductive material is 8.3S / cm, and the stretchable length is 210%. The conductivity of the high-conductive layer is 5263S / cm, and the elongation at break is 2%. The width of each annular protrusion structure on the surface of the high-conductive layer is 600μm, and the protrusion height is 300μm.

[0102] Figure 6 Schematic diagram of high fatigue threshold for TPM-functionalized silica particles and poly(ethyl acrylate) polymers. Entanglement refers to the physical interweaving and interlacing between polymer chains or between different molecules within a chain. These interlacings are not covalent bonds, but physical interlacing of chains. Crosslinking refers to the covalent bonds formed in the polymer chain, which bind different polymer chains or segments together. When a crack strikes a polymer chain, the number of interchain entanglements in the polymer used greatly exceeds the crosslinks. The dense entanglement transfers the tension in the polymer chain to many other chains along its length. The sparse crosslinks prevent the polymer chain from unravelling, and the low friction between the polymer chains causes the stress to be dispersed throughout the polymer chain. When hitting the particle cluster, the strong polymer-particle adhesion transfers the high stress from the polymer to the particle. Because the particles are rigid, the stress is dispersed to many particle-particle gaps in the cluster. The multi-scale stress dispersion greatly improves the fatigue threshold.

[0103] like Figure 7 As shown, when small cracks appear in the inner core due to long-term use, the stress at the crack tip is dispersed under the large shear action of the soft matrix. As the crack tip expands, the stress of the hard fiber is concentrated and the crack is blocked by the hard fiber, which greatly alleviates the expansion of the small crack.

[0104] Figure 8 The schematic diagram of the composite conductive material of polypyrrole and graphene oxide. PPy with π bonds on the pyrrole ring can be adsorbed on the surface of graphene oxide through π-π stacking interaction, hydrogen bonding and van der Waals interaction. Due to the strong π-π interaction, polypyrrole is more likely to move carriers, thereby increasing conductivity. The high specific surface area of ​​graphene oxide allows pyrrole monomers to be fully adsorbed on its surface, inhibiting the aggregation of pyrrole.

[0105] Fig. 9 This is a schematic diagram of the controllable regularly distributed cracks in the high conductive layer of the sensor under tension. It can be seen from the figure that: no cracks occur in the high conductive layer in the initial state; when a longitudinal tensile force is applied to the sensor, the stress on the high conductive layer will be concentrated at both ends of the link, causing cracks to occur at these stress concentration points.

[0106] Fig.10The sensing mechanism and local conductive path schematic diagram of the strain sensor prepared in this embodiment. It can be seen that the main transmission path of electrons before pre-stretching is the high conductive layer of the sensor. After the sensor is pre-stretched, cracks are generated in the stress concentration area of ​​the high conductive layer. At this time, the transmission path of electrons is from the low conductive fiber to the high conductive outer layer, and so on. It is equivalent to connecting several low-resistance inner cores and high-resistance outer layers in series. Therefore, when the sensor is strained, the crack gap increases, resulting in an increase in the sensor resistance, which effectively improves the sensing performance of the sensor. In the figure, R represents the resistance of the high conductive film layer when not stretched, and R' refers to the resistance of the low conductive inner core when not stretched, and R is much smaller than R'. R 1 , R 2 , R 3 They represent the resistance of each section separated by the crack in the high conductive film layer after the crack is generated, R 1 '、R 2 ' respectively refer to the resistance of the current transmitted through the low conductive core at the crack after the crack is generated, R 1 '、R 2 ' is much larger than R 1 , R 2 , R 3 .

[0107] Fig.11 The result curve of the stress-strain test of the strain sensor prepared in this embodiment shows that the elongation at break of the sensor can reach 120%, which means that the sensor has good stretchability and can fully meet the needs of the wearable field of the human body.

[0108] Fig.12 From the strain resistance variation characteristic curve of the strain sensor prepared in this embodiment, it can be seen that: when the strain is in the range of 0-20%, the sensor sensitivity coefficient GF is about 675.06; when the strain range is 20-40%, the sensitivity coefficient GF is about 314.2.

[0109] Fig.13 The resistance change characteristic curve of the strain sensor prepared in this embodiment during the cyclic loading and releasing process shows that the resistance of the sensor does not shift significantly when it is repeatedly loaded and released with different strains, indicating the good stability of the sensor under different strains.

[0110] Fig.14 The strain sensor prepared in this embodiment was subjected to a step test, and the result showed that the sensor had a very small creep effect under a tensile strain of 0% to 40% and a strain step of 5%.

[0111] Fig.15The strain sensor prepared in this embodiment was subjected to 3000 cycles of loading / unloading (strain range 0% to 30%) to test the electrical stability and repeatability of the sensor. It can be seen that after 3000 cycles of testing, the sensor has stable electrical characteristics, thus proving that the sensor has good consistency.

[0112] The above description is only an exemplary embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. Anti-fatigue flexible strain sensor based on multi-scale stress dispersion mechanism, characterized by: It includes a low-conductivity inner core, a high-conductivity layer and a packaging layer which are sequentially arranged from the inside to the outside; The low-conductivity inner core comprises a flexible substrate with a cylindrical structure; the surface of the flexible substrate is uniformly provided with grooves along the circumferential direction, the grooves penetrate along the axial direction of the flexible substrate, and the cross-section is rectangular; each groove of the flexible substrate is filled with a low-conductivity material, and the low-conductivity material is consistent with the shape of the groove; the low-conductivity inner core is formed by the flexible substrate equipped with the low-conductivity material; The high-conductivity layer is cylindrical and covers the surface of the low-conductivity inner core; the surface of the high-conductivity layer is evenly distributed with a number of annular protrusion structures along the axial direction; The packaging layer is coated on the surface of the high conductive layer, so that the flexible strain sensor has a cylindrical long strip structure as a whole.

2. The flexible strain sensor according to claim 1, characterized in that: The flexible substrate and the encapsulation layer are prepared from silica nanoparticles functionalized with polyethyl acrylate and 3-(trimethoxysilyl)propyl methacrylate.

3. The flexible strain sensor according to claim 1 or 2, characterized in that: The diameter of the flexible substrate is 500 μm to 1 mm, and the stretchable length is not less than 200%. The number of grooves uniformly distributed along the circumference of the flexible substrate is 5 to 10.

4. The flexible strain sensor according to claim 1, characterized in that: The low-conductivity material is made of polyethyl acrylate, 3-(trimethoxysilyl)propyl methacrylate functionalized silica nanoparticles and polypyrrole.

5. The flexible strain sensor according to claim 1 or 4, characterized in that: The low-conductive material has an electrical conductivity of no more than 10 S / cm and a stretchable length of no less than 200%.

6. The flexible strain sensor according to claim 1, characterized in that: The high conductive layer is prepared from polypyrrole, graphene oxide and phytic acid.

7. The flexible strain sensor according to claim 1 or 6, characterized in that: The electrical conductivity of the highly conductive layer is not less than 4000 S / cm, and the elongation at break is not greater than 2%.

8. The flexible strain sensor according to claim 1, characterized in that: The width of each annular protrusion structure on the surface of the highly conductive layer is 400-800 μm, and the protrusion height is 100-400 μm. The junction between each annular protrusion structure and the surface of the highly conductive layer is formed with an annular crack extending along the circumference of the highly conductive layer by pre-stretching.

9. A method for preparing an anti-fatigue flexible strain sensor based on a multi-scale stress dispersion mechanism according to any one of claims 1 to 8, characterized in that: The steps include: Step 1: Prepare flexible substrate and encapsulation layer slurry The silica nanoparticles functionalized with 3-(trimethoxysilyl)propyl methacrylate and the monomer ethyl acrylate are uniformly mixed in N,N-dimethylformamide, tricyclo[5.2.1.02,6]decanedioic acid diacrylate as a crosslinking agent and 2-hydroxy-2-methylpropiophenone as a photoinitiator are added, and the mixture is stirred at room temperature to obtain a flexible matrix and an encapsulation layer slurry; wherein the ratio of the mass of the nanoparticles to the volume of ethyl acrylate is 0.4-0.6 g:1 mL, and the molar ratio of the crosslinking agent to the monomer is 10 -4 ~10 -3 : 1, the molar ratio of the photoinitiator to the crosslinking agent is 0.3-0.4:1; Step 2: Prepare low conductive material slurry 3-(trimethoxysilyl) propyl methacrylate functionalized silica nanoparticles and monomer ethyl acrylate are mixed evenly in N,N-dimethylformamide, tricyclo[5.2.1.02,6]decanedioic acid diacrylate as a crosslinking agent and 2-hydroxy-2-methylpropiophenone as a photoinitiator are added, stirred at room temperature for reaction, and then polypyrrole is added and ultrasonically mixed evenly to obtain a low conductive material slurry; wherein: the ratio of the mass of the nanoparticles to the volume of ethyl acrylate is 0.7-0.9 g: 1 mL; the molar ratio of the crosslinking agent to the monomer is 10 -4 ~10 -3 : 1, the molar ratio of the photoinitiator to the crosslinking agent is 0.3-0.4:1; the mass ratio of the nanoparticles to the polypyrrole is 1600-1700:1; Step 3: Prepare high conductive layer slurry The graphene oxide nanosheets are dispersed in water, pyrrole is added and mixed evenly, and FeCl3-6H2O is added to carry out stirring polymerization reaction at 0-4°C. The obtained product is filtered, washed and vacuum dried to obtain a polypyrrole / graphene oxide nanocomposite material; wherein the amount ratio of the graphene oxide nanosheets, FeCl3-6H2O and pyrrole is 15-20 mg: 0.3-0.4 g: 30 μL; Ultrasonic dispersion of polypyrrole / graphene oxide nanocomposite in phytic acid solution to obtain high conductive layer slurry; wherein the amount ratio of polypyrrole / graphene oxide nanocomposite to phytic acid is 100-110 g:1 mol; Step 4: Prepare the sensor by using a casting process combined with mold forming The flexible substrate and the encapsulation layer slurry are poured into the substrate mold and UV-cured to form a flexible substrate with grooves uniformly distributed on the surface along the circumferential direction; the low-conductive material slurry is then injected into the grooves of the flexible substrate and UV-cured to form a low-conductive inner core; the low-conductive inner core is repeatedly stretched 2000-3000 times under a strain of 15-30% to stabilize the microstructure of the inner core; The low-conductivity inner core is straightened and suspended and positioned at the central axis of the high-conductivity mold, the high-conductivity layer slurry is cast into the high-conductivity layer mold to wrap the inner core, and then the bubbles are removed by vacuum, infrared curing and drying are carried out; the device is taken out and repeatedly stretched 10 to 50 times at a strain of 15 to 30%, so that the high-conductivity layer forms regular annular cracks extending along the circumference of the high-conductivity layer at the junction of each annular protrusion structure and the surface of the high-conductivity layer; two wires are fixed at both ends of the axial direction of the high-conductivity layer; The prepared device is straightened and suspended in the center of a cylindrical packaging layer mold, and then the flexible substrate and packaging layer slurry are poured into the packaging layer mold and UV-cured to obtain a fatigue-resistant flexible strain sensor based on a multi-scale stress dispersion mechanism.

Citation Information

Patent Citations

  • Bionic flexible actuator having real-time feedback function and preparation method thereof

    CN109921679A

  • Three-dimensional force sensor and measuring system for minimally invasive surgery

    CN115290243A

  • PEDOT: PSS-based flexible strain sensor and preparation method thereof

    CN115993086A

  • Wireless passive strain sensing yarn for monitoring limb movement state and preparation method thereof

    CN116999055A

  • Methods and sensors for detecting strain and stress

    US6079277A

Cited By

  • Multidirectional flexible sensor and preparation method thereof

    CN119779364A