Ultrasonic detection method for supporting frame casting shaft hole position
By using ultrasonic comparison test blocks and ultrasonic flaw detectors, the metallurgical quality missed detection problem caused by complex structures in X-ray detection is solved, and efficient and accurate detection of the shaft hole position of the supporting frame castings is achieved.
Patent Information
- Application Number
- CN202411093135.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-26
AI Technical Summary
During X-ray detection, the complex structure supporting frame castings leads to shading of the ray beam at the intersection of surrounding panels and ribs, resulting in distortion and edge corrosion of the transilluminated negative film, unable to accurately display the internal metallurgical quality, and there is a missed inspection.
Ultrasonic comparison test blocks are used for testing. By making ultrasonic comparison test blocks with the same material and structure as those of the supporting frame castings, artificial defects are prepared and detection sensitivity is adjusted. Ultrasonic flaw detectors are used for testing to ensure that metallurgical defects in the shaft hole can be accurately detected.
Through ultrasonic detection methods, metallurgical defects supporting the shaft hole position of the frame casting can be efficiently and accurately detected, avoiding missed inspection and ensuring the reliability of metallurgical quality.
Smart Images

Figure CN119023819A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nondestructive testing of castings, and in particular to an ultrasonic testing method for supporting the position of an axial hole of a frame casting. Background Art
[0002] Figure 1 The support frame on the aircraft engine is shown, and the support frame is formed by casting. The casting of the support frame is provided with two tube bodies 1, and an axial hole 2 is formed inside each tube body 1. The two tube bodies 1 and the rib plates on the outer wall of the tube body 1 have the same structure shape, but the positions differ by 180 degrees. Specifically, two outer panels 3 and inner panels 4 are integrally formed on the outer wall of each tube body 1, which are spaced apart from each other; an upper rib plate 5 and a lower rib plate 6 are arranged between the outer panel 3, the inner panel 4 and the outer wall surface of the tube body 1; the outer panel 3 and the inner panel 4 are arranged at an angle to each other, and the upper rib plate 5 is located at the position where the distance between the outer panel 3 and the inner panel 4 is the smallest, and the lower rib plate 6 is located at the position where the distance between the outer panel 3 and the inner panel 4 is the largest; a reinforcing rib 7 is also arranged between the outer side surface of the outer panel 3 and the outer wall surface of the tube body 1, and the reinforcing rib 7 and the upper rib plate 5 are respectively located on both sides of the outer panel 3. The internal metallurgical quality of the axial hole 1 in the support frame is mainly guaranteed by X-ray detection technology.
[0003] Due to the complex structure of the casting of the support frame, the panels and ribs around this position block the radiation beam during X-ray inspection, resulting in distortion of the radiographic films at the intersection of the ribs and panels. In addition, since these intersections are multi-walled structures with variable cross-sections, there is also edge erosion in the radiographic films of these areas, making it impossible to display the internal metallurgical quality on the film, resulting in missed inspections. Summary of the invention
[0004] The main purpose of the present invention is to propose an ultrasonic detection method for the position of the shaft hole of a support frame casting, aiming to solve the above technical problems.
[0005] To achieve the above object, the present invention provides an ultrasonic detection method for the position of the shaft hole of a support frame casting, comprising the following steps:
[0006] S1. Prepare ultrasonic comparison test blocks;
[0007] S2, verification of ultrasonic comparison test blocks;
[0008] S3, adjustment of ultrasonic detection sensitivity and transmission correction;
[0009] S4. Use ultrasonic waves to inspect the support frame casting.
[0010] Preferably, in step S1, the steps of making the ultrasonic contrast test block include:
[0011] S101. The same material and the same process as the support frame casting are used for casting. The ultrasonic comparison test block has a tube body, an outer panel, an inner panel, an upper rib plate, a lower rib plate and reinforcing ribs corresponding to the upper structure of the support frame casting, and an axial hole is formed inside the tube body;
[0012] S102, polishing and grinding the ultrasonic comparison test block to make its surface roughness reach the casting acceptance requirement Ra = 3.2μm;
[0013] S103, preparing artificial defects at the transition fillet positions of the root of the lower rib plate, the upper rib plate, and the reinforcing ribs.
[0014] Preferably, in step S103, the artificial defect is a flat-bottomed blind hole formed by drilling from the outer wall of the tube body in a radial direction toward the inner wall, and the diameter of the blind hole includes φ0.8 mm and φ1.2 mm.
[0015] Preferably, the center of the blind hole is 20 mm away from the center of the lower rib plate, or the upper rib plate, or the reinforcing rib at its corresponding position.
[0016] Preferably, the depth of the blind hole includes a hole depth of 3 mm and a hole bottom distance of 3 mm from the inner wall of the tube body; the artificial defects include artificial defects near the surface and artificial defects far from the surface, the artificial defects near the surface are blind holes with the hole bottom being 3 mm away from the inner wall of the tube body; the artificial defects far from the surface are blind holes with a hole depth of 3 mm.
[0017] Preferably, in step S3, the steps of adjusting the ultrasonic detection sensitivity and correcting the transmission include:
[0018] S301. Detect near-surface artificial defects on the ultrasonic comparison test block by adjusting the gain button of the ultrasonic flaw detector, so that the defect wave height reaches 80% of the ultrasonic display, and record these gain values respectively; then select a position with uniform wall thickness in the axial hole of the ultrasonic comparison test block for detection, and adjust the gain button to make the bottom wave height reach 80% of the observation interface, and then place the ultrasonic flaw detector at this gain at the same thickness position of the axial hole of the support frame casting, and observe the difference in wave height between the two at this time; if the bottom wave on the support frame casting is higher than the bottom wave of the ultrasonic comparison test block, reduce the gain so that the wave height reaches 80% of the observation interface, and record the reduced gain at this time. The gain value is calculated, and the maximum gain value previously adjusted on the ultrasonic comparison test block for detecting artificial defects near the surface is subtracted from the gain value reduced at this time to obtain a first gain value, and the first gain value is used as the gain value for detecting defects near the surface of the shaft hole of the support frame casting this time; if the bottom wave height on the support frame casting is lower than the bottom wave of the ultrasonic comparison test block, the gain is increased so that the wave height reaches 80% of the observation interface, and the increased gain value is recorded at this time, and the maximum gain value previously adjusted on the ultrasonic comparison test block for detecting artificial defects near the surface is added to the gain value increased at this time to obtain the first gain value, and the first gain value is used as the gain value for detecting defects near the surface of the shaft hole of the support frame casting this time;
[0019] S302. Detect the artificial defects on the far surface of the ultrasonic comparison test block by adjusting the gain button of the ultrasonic flaw detector, so that the wave height of the defect wave reaches 80% of the ultrasonic display, and record these gain values respectively; then select a position with uniform wall thickness in the axial hole of the ultrasonic comparison test block for detection, and adjust the gain button to make the bottom wave wave height reach 80% of the observation interface, and then place the ultrasonic flaw detector at this gain at the same thickness position of the axial hole of the support frame casting, and observe the difference in wave height between the two at this time; if the bottom wave on the support frame casting is higher than the bottom wave of the ultrasonic comparison test block, reduce the gain so that the wave height reaches 80% of the observation interface, and record the reduced gain at this time. The gain value is calculated, and the maximum gain value previously adjusted on the ultrasonic comparison test block for detecting artificial defects on the far surface is subtracted from the reduced gain value at this time to obtain a second gain value, and the second gain value is used as the gain value for detecting defects on the far surface of the shaft hole of the support frame casting this time; if the bottom wave height on the support frame casting is lower than the bottom wave of the ultrasonic comparison test block, the gain is increased so that the wave height reaches 80% of the observation interface, and the increased gain value at this time is recorded, and the maximum gain value previously adjusted on the ultrasonic comparison test block for detecting artificial defects on the far surface is added to the increased gain value at this time to obtain a second gain value, and the second gain value is used as the gain value for detecting defects on the far surface of the shaft hole of the support frame casting this time.
[0020] Preferably, in step S4, the support frame casting is inspected, including the following steps:
[0021] S401, adjusting the gain of the ultrasonic flaw detector to the first gain value in step S301, tightly coupling the ultrasonic probe to the detected position of the shaft hole of the support frame casting, scanning the shaft hole of the support frame casting at a speed of no more than 50 mm / s using a longitudinal wave vertical incidence method, detecting the internal metallurgical defects near the surface of the shaft hole, and judging whether there are excessive defects in the detection area by observing the change of its waveform;
[0022] S402, adjusting the gain of the ultrasonic flaw detector to the second gain value in step S302, tightly coupling the ultrasonic probe to the detected position of the shaft hole of the support frame casting, using the longitudinal wave vertical incidence method to scan the shaft hole of the support frame casting at a speed not exceeding 50 mm / s, detecting the internal metallurgical defects at the far surface of the shaft hole, and judging whether there are excessive defects in the detection area by observing the changes in its waveform.
[0023] Preferably, in the steps S2 to S4, an ultrasonic probe with a frequency of 10 MHz and a size of 0.25 In is selected; and the equipment used is an ultrasonic flaw detector of model USM33LEMO.
[0024] Preferably, two artificial defect blind holes are prepared at the root transition fillet positions on both sides of the lower rib plate, namely artificial defect A, artificial defect B, artificial defect C and artificial defect D, wherein:
[0025] Artificial defect A is a blind hole with a hole diameter of φ0.8 mm and a hole depth of 3 mm;
[0026] Artificial defect B is a blind hole with a hole diameter of φ0.8mm and a bottom distance of 3mm from the inner wall of the tube body;
[0027] Artificial defect C is a blind hole with a hole diameter of φ1.2mm and a hole depth of 3mm;
[0028] Artificial defect D is a blind hole with a hole diameter of φ1.2mm and a bottom distance of 3mm from the inner wall of the tube body;
[0029] Artificial defects B and D are located on the left side of the lower rib plate, both 20 mm away from the center of the lower rib plate; the distance between artificial defect B and the inner panel is 30 mm; the distance between artificial defect D and the inner panel is 55 mm;
[0030] Artificial defect A and artificial defect C are located on the right side of the lower rib plate; both are 20 mm away from the center of the lower rib plate; the distance between artificial defect A and the inner panel is 30 mm; the distance between artificial defect C and the inner panel is 55 mm.
[0031] Preferably, an artificial defect blind hole is prepared at the root transition fillet position on both sides of the reinforcing rib, which are respectively artificial defect E and artificial defect F; an artificial defect blind hole is prepared at the root transition fillet position on both sides of the upper rib plate, which are respectively artificial defect G and artificial defect H;
[0032] Artificial defect E is a blind hole with a hole diameter of φ0.8 mm and a hole depth of 3 mm;
[0033] The artificial defect F is a blind hole with a hole diameter of φ0.8 mm and a bottom of the hole 3 mm away from the inner wall of the tube body (1);
[0034] The artificial defect G is a blind hole with a hole diameter of φ1.2mm and a hole depth of 3mm;
[0035] The artificial defect H is a blind hole with a hole diameter of φ1.2 mm and a bottom of the hole 3 mm away from the inner wall of the tube body (1);
[0036] The artificial defect E is located on the right side of the reinforcing rib, and the artificial defect F is located on the left side of the reinforcing rib; the artificial defect E and the artificial defect F are 20 mm away from the center of the reinforcing rib, and 20 mm away from the outer panel, respectively;
[0037] The artificial defect H is located on the right side of the upper rib plate, and the artificial defect G is located on the left side of the upper rib plate; the artificial defect H and the artificial defect G are respectively 20 mm away from the center of the upper rib plate and 19 mm away from the outer panel.
[0038] Due to the adoption of the above technical solution, the beneficial effects of the present invention are as follows:
[0039] (1) In the present invention, an ultrasonic comparison test block is used to adjust the ultrasonic detection sensitivity and perform transmission correction. Since the location of the artificial defect of the ultrasonic comparison test block is at a position that is relatively representative of the detection area and easy to prepare, it is easy to operate and can accurately adjust the detection parameters when performing sensitivity adjustment and transmission correction, thereby ensuring that when the product is subjected to ultrasonic testing, the metallurgical defects inside it can be detected efficiently and accurately, thereby avoiding the occurrence of missed detection.
[0040] (2) The ultrasonic comparison test blocks are processed with φ0.8mm and φ1.2mm flat-bottomed blind holes on the near and far surfaces of the detection area. They can efficiently and accurately detect single or multiple hole defects with a diameter greater than or equal to 0.8mm at the shaft hole position of the support frame casting, avoid missed detection, and ensure the metallurgical quality of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0042] Figure 1 This is a schematic diagram of the structure of the support frame casting on the aircraft engine;
[0043] Figure 2 Schematic diagram of the ultrasonic comparison test block structure Figure 1 ;
[0044] Figure 3 Schematic diagram of the ultrasonic comparison test block structure Figure 2 ;
[0045] Figure 4 Schematic diagram of surface roughness comparison test block;
[0046] Figure 5 It is a schematic diagram of the far surface ultrasonic waveform;
[0047] Figure 6 It is a schematic diagram of the far surface ultrasonic waveform;
[0048] Figure 7 Schematic diagram of ultrasonic testing of the shaft hole position of the support frame casting.
[0049] Explanation of the accompanying figures: 1. Tube body; 2. Axial hole; 3. Outer panel; 4. Inner panel; 5. Upper rib plate; 6. Lower rib plate; 7. Reinforcing rib; 8. Ultrasonic comparison test block. DETAILED DESCRIPTION
[0050] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0052] As shown in the accompanying drawings, a specific embodiment of an ultrasonic detection method for the position of an axial hole of a support frame casting provided by the present invention includes the following steps:
[0053] S1, making an ultrasonic comparison test block 8;
[0054] S2, verification of ultrasonic comparison test block 8;
[0055] S3, adjustment of ultrasonic detection sensitivity and transmission correction;
[0056] S4. Use ultrasonic waves to inspect the support frame casting.
[0057] Combination Figure 2 , Figure 3 As shown, in step S1, the steps of making the ultrasonic comparison test block 8 include:
[0058] S101, using the same material and the same process as the support frame casting to cast, the ultrasonic comparison test block 8 has a tube body 1, an outer panel 3, an inner panel 4, an upper rib plate 5, a lower rib plate 6 and a reinforcing rib 7 corresponding to the structure on the support frame casting, and an axial hole 2 is formed inside the tube body 1;
[0059] S102, polishing and grinding the ultrasonic comparison test block 8 with a rubber grinding head, and comparing with a surface roughness comparison test block, requiring the surface roughness of the ultrasonic comparison test block 8 to meet the casting acceptance requirement Ra = 3.2 μm;
[0060] S103, artificial defects are prepared at the root transition fillet positions of the lower rib plate 6, the upper rib plate 5, and the reinforcing rib 7. In this embodiment, the ultrasonic detection of the axial hole position of the support frame casting requires detection within 25 mm on both sides of the corresponding rib plate and rib. Therefore, the center of the blind hole is 20 mm away from the center of the lower rib plate 6, or the upper rib plate 5, or the reinforcing rib 7 at its corresponding position.
[0061] Since the variable cross section is within 19mm from the corresponding ribs and ribs, it is very difficult to prepare the artificial defect in this area. Therefore, the artificial defect cannot be prepared in this area. Within 21mm to 25mm from the corresponding ribs and ribs, the test surface is approximately a plane. Preparing the artificial defect in this area is not representative for the test surface. Therefore, after comprehensive consideration, it is determined that the artificial defect is prepared 20mm from the center of the lower rib 6, or the upper rib 5, or the reinforcing rib 7.
[0062] Since the acceptance criteria for the support frame castings require that a single hole-type defect does not exceed an equivalent flat-bottom hole of φ1.2mm. In addition, some products of the support frame castings have internal metallurgical defects of φ0.8mm. After machining, the defect is located on the surface of the product. When the fluorescent penetration test is performed, it is judged as a surface defect and does not meet the standard requirements. Therefore, in the present embodiment, in the step S103, the artificial defect is a flat-bottomed blind hole formed by drilling from the outer wall of the tube body 1 in the radial direction toward the inner wall, and the diameters of the blind holes include φ0.8mm and φ1.2mm. The artificial defect blind hole with a diameter of φ0.8mm is set at the position where defects often occur, that is, the transition fillet position of the root of the lower rib plate 6, the upper rib plate 5, and the reinforcing rib 7. The artificial defect blind hole of φ0.8mm is set mainly to detect the existence of internal metallurgical defects of φ0.8mm in the product.
[0063] In this embodiment, the depth of the blind hole includes a hole depth of 3 mm and a hole bottom distance of 3 mm from the inner wall of the tube body 1; the artificial defects include near-surface artificial defects and far-surface artificial defects, specifically: the near-surface artificial defect is a blind hole with a hole bottom distance of 3 mm from the inner wall of the tube body 1; the far-surface artificial defect is a blind hole with a hole depth of 3 mm. Furthermore, the near-surface and far-surface are distinguished by the distance between the hole bottom and the inner wall of the tube body 1.
[0064] Specific combination Figure 2 and Figure 3 As shown, A, B, C, D, E, F, G, and H indicate the locations of artificial defects.
[0065] Combination Figure 2 As shown, two artificial defect blind holes are prepared at the root transition fillet positions on both sides of the lower rib plate 6, namely artificial defect A, artificial defect B, artificial defect C and artificial defect D, wherein:
[0066] Artificial defect A is a blind hole with a hole diameter of φ0.8 mm and a hole depth of 3 mm;
[0067] Artificial defect B is a blind hole with a hole diameter of φ0.8 mm and a bottom distance of 3 mm from the inner wall of the tube body 1;
[0068] Artificial defect C is a blind hole with a hole diameter of φ1.2mm and a hole depth of 3mm;
[0069] The artificial defect D is a blind hole with a hole diameter of φ1.2 mm and a bottom distance of 3 mm from the inner wall of the tube body 1.
[0070] Artificial defects A and C are artificial defects on the far surface, and artificial defects B and D are artificial defects on the near surface.
[0071] Artificial defects B and D are located on the left side of the lower rib plate 6, both 20 mm away from the center of the lower rib plate 6; the distance between artificial defect B and the inner panel 4 is 30 mm; the distance between artificial defect D and the inner panel 4 is 55 mm;
[0072] Artificial defect A and artificial defect C are located on the right side of the lower rib plate 6; both are 20 mm away from the center of the lower rib plate 6; the distance between artificial defect A and the inner panel 4 is 30 mm; the distance between artificial defect C and the inner panel 4 is 55 mm.
[0073] Combination Figure 3 As shown, an artificial defect blind hole is prepared at the root transition fillet position on both sides of the reinforcing rib 7, which are artificial defects E and F respectively; an artificial defect blind hole is prepared at the root transition fillet position on both sides of the upper rib plate 5, which are artificial defects G and H respectively;
[0074] Artificial defect E is a blind hole with a hole diameter of φ0.8 mm and a hole depth of 3 mm;
[0075] The artificial defect F is a blind hole with a hole diameter of φ0.8 mm and a bottom distance of 3 mm from the inner wall of the tube body 1;
[0076] The artificial defect G is a blind hole with a hole diameter of φ1.2mm and a hole depth of 3mm;
[0077] The artificial defect H is a blind hole with a hole diameter of φ1.2mm and a bottom distance of 3mm from the inner wall of the tube body 1;
[0078] Artificial defects E and G are artificial defects on the far surface, and artificial defects F and H are artificial defects on the near surface.
[0079] The artificial defect E is located on the right side of the reinforcing rib 7, and the artificial defect F is located on the left side of the reinforcing rib 7; the artificial defect E and the artificial defect F are 20 mm away from the center of the reinforcing rib 7, and 20 mm away from the outer panel 3, respectively;
[0080] The artificial defect H is located on the right side of the upper rib plate 5, and the artificial defect G is located on the left side of the upper rib plate 5; the artificial defect H and the artificial defect G are respectively 20 mm away from the center of the upper rib plate 5, and are respectively 19 mm away from the outer panel 3.
[0081] In step S2 and step S4, an ultrasonic probe with a frequency of 10MHz and a size of 0.25In is selected; the equipment used is an ultrasonic flaw detector of model USM33LEMO. Ultrasonic waves are used to detect the support frame casting. Since the density of the casting itself is not very high, the attenuation of ultrasonic waves is relatively large, so a probe with a higher frequency cannot be used; but for ultrasonic detection, the higher the frequency of the probe, the better the ultrasonic detection effect. Considering these two factors, a probe with a frequency of 10MHz is selected. Since the inner wall of the shaft hole 2 is an arc structure, when performing ultrasonic detection, the coupling performance between the probe and the detection surface also affects the ultrasonic detection result. Therefore, it is necessary to ensure the coupling performance between the probe and the detection surface. Therefore, the size of the ultrasonic probe should be small, so an ultrasonic probe with a size of 0.25In is selected.
[0082] In step S3, the steps of adjusting the ultrasonic detection sensitivity and correcting the transmission include:
[0083] S301. Detect near-surface artificial defects on the ultrasonic comparison test block 8 by adjusting the gain button of the ultrasonic flaw detector, that is, detect artificial defects B, D, F, and H, so that the defect wave height reaches 80% of the ultrasonic display, and record these gain values respectively, specifically: 58dB, 61dB, 61.5dB, and 57dB; then select a position with uniform wall thickness in the axial hole 2 of the ultrasonic comparison test block 8 for detection, specifically, select a position with a wall thickness of 25mm for detection, and adjust the gain button to make the bottom wave height reach 80% of the observation interface, and then place the ultrasonic flaw detector under this gain on the support frame casting. At the same thickness position of the axial hole of the supporting frame casting, observe the difference in wave heights between the two at this time. At this time, the bottom wave on the supporting frame casting is higher than the bottom wave of the ultrasonic comparison test block 8. Reduce the gain so that the wave height reaches 80% of the observation interface, and record the reduced gain value at this time. Specifically, the reduced gain value is 3dB, and the maximum gain value previously adjusted on the ultrasonic comparison test block 8 for detecting near-surface artificial defects is subtracted from the reduced gain value at this time to obtain the first gain value, that is, 61.5dB-3dB=58.5dB, and the first gain value of 58.5dB is used as the gain value for detecting defects at the near-surface position of the axial hole of the supporting frame casting this time.
[0084] S302, by adjusting the gain button of the ultrasonic flaw detector, the artificial defects on the far surface of the ultrasonic comparison test block 8 are detected, that is, the artificial defects A, C, E, and G are detected, so that the wave height of the defect wave reaches 80% of the ultrasonic display, and these gain values are recorded respectively, specifically: 61dB, 70.5dB, 68.5dB, and 57dB; then a position with uniform wall thickness is selected in the axial hole 2 of the ultrasonic comparison test block 8 for detection, and the gain button is adjusted to make the bottom wave height reach 80% of the observation interface, and then the ultrasonic flaw detector under this gain is placed at the same thickness position of the axial hole of the support frame casting, and the observation is performed. Observe the difference in wave heights between the two at this time. At this time, the bottom wave on the support frame casting is higher than the bottom wave of the ultrasonic comparison test block 8. Reduce the gain so that the wave height reaches 80% of the observation interface, and record the reduced gain value at this time. Specifically, the reduced gain value is 2dB, and the maximum gain value previously adjusted on the ultrasonic comparison test block 8 to detect artificial defects on the far surface is subtracted from the reduced gain value at this time to obtain the second gain value, that is, 70.5dB-2dB=68.5dB, and the second gain value of 68.5dB is used as the gain value for detecting defects on the far surface of the shaft hole of the support frame casting this time.
[0085] In step S4, the support frame casting is inspected, including the following steps:
[0086] S401, adjusting the gain of the ultrasonic flaw detector to the first gain value of 58.5 dB in step S301, tightly coupling the ultrasonic probe to the detected position of the shaft hole of the support frame casting, scanning the shaft hole of the support frame casting at a speed of no more than 50 mm / s using the longitudinal wave vertical incidence method, detecting the internal metallurgical defects near the surface of the shaft hole, and judging whether there are excessive defects in the detection area by observing the changes in its waveform;
[0087] S402, adjusting the gain of the ultrasonic flaw detector to the second gain value of 68.5 dB in step S302, tightly coupling the ultrasonic probe to the detected position of the shaft hole of the support frame casting, using the longitudinal wave vertical incidence method to scan the shaft hole of the support frame casting at a speed not exceeding 50 mm / s, and detecting the internal metallurgical defects at the far surface of the shaft hole, and judging whether there are excessive defects in the detection area by observing the changes in its waveform.
[0088] Specifically, in this embodiment, in step S401, the longitudinal wave vertical incidence method is used to scan the shaft hole of the support frame casting at a speed of 3 mm / s. In step S402, the longitudinal wave vertical incidence method is used to scan the shaft hole of the support frame casting at a speed of 10 mm / s.
[0089] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. An ultrasonic detection method for the position of the shaft hole of a support frame casting, characterized in that: The following steps are involved: S1. preparing an ultrasonic comparison test block (8); S2, verification of ultrasonic comparison test block (8); S3, adjustment of ultrasonic detection sensitivity and transmission correction; S4. Use ultrasonic waves to inspect the support frame casting.
2. An ultrasonic detection method for the position of the shaft hole of a support frame casting according to claim 1, characterized in that: In step S1, the steps of making the ultrasonic comparison test block (8) include: S101. The same material and the same process as the support frame casting are used for casting. The ultrasonic comparison test block (8) has a tube body (1), an outer panel (3), an inner panel (4), an upper rib plate (5), a lower rib plate (6) and reinforcing ribs (7) corresponding to the structure on the support frame casting. An axial hole (2) is formed inside the tube body (1); S102, polishing and grinding the ultrasonic comparison test block (8) to make its surface roughness reach the casting acceptance requirement Ra=3.2 μm; S103, artificial defects are prepared at the root transition fillet positions of the lower rib plate (6), the upper rib plate (5), and the reinforcing rib (7).
3. An ultrasonic detection method for the position of the shaft hole of a support frame casting according to claim 2, characterized in that: In step S103, the artificial defect is a flat-bottomed blind hole formed by drilling from the outer wall of the tube body (1) in a radial direction toward the inner wall, and the diameter of the blind hole includes φ0.8 mm and φ1.2 mm.
4. The ultrasonic detection method for the position of the shaft hole of the support frame casting according to claim 2, characterized in that: The distance between the center of the blind hole and the center of the lower rib plate (6), or the upper rib plate (5), or the reinforcing rib (7) at the corresponding position is 20 mm.
5. The ultrasonic detection method for the position of the shaft hole of the support frame casting according to claim 3, characterized in that: The depth of the blind hole includes a hole depth of 3 mm and a hole bottom distance of 3 mm from the inner wall of the tube body (1); the artificial defects include artificial defects near the surface and artificial defects far from the surface, the artificial defects near the surface are blind holes with a hole bottom distance of 3 mm from the inner wall of the tube body (1); the artificial defects far from the surface are blind holes with a hole depth of 3 mm.
6. An ultrasonic detection method for the position of the shaft hole of a support frame casting according to claim 5, characterized in that: In step S3, the steps of adjusting the ultrasonic detection sensitivity and correcting the transmission include: S301. Detect near-surface artificial defects on the ultrasonic comparison test block (8) by adjusting the gain button of the ultrasonic flaw detector, so that the defect wave height reaches 80% of the ultrasonic display, and record these gain values respectively; then select a position with uniform wall thickness in the axial hole (2) of the ultrasonic comparison test block (8) for detection, and adjust the gain button so that the bottom wave height reaches 80% of the observation interface, and then place the ultrasonic flaw detector at this gain at the same thickness position of the axial hole of the support frame casting, and observe the difference in wave height between the two at this time; if the bottom wave on the support frame casting is higher than the bottom wave of the ultrasonic comparison test block (8), reduce the gain so that the wave height reaches 80% of the observation interface, and record the reduced gain at this time. The gain value is obtained by subtracting the reduced gain value at this time from the maximum gain value previously adjusted on the ultrasonic comparison test block (8) for detecting artificial defects near the surface, and obtaining a first gain value, and using the first gain value as the gain value for detecting defects near the surface of the shaft hole of the support frame casting this time; if the bottom wave height on the support frame casting is lower than the bottom wave of the ultrasonic comparison test block (8), then the gain is increased so that the wave height reaches 80% of the observation interface, and the increased gain value at this time is recorded, and the maximum gain value previously adjusted on the ultrasonic comparison test block (8) for detecting artificial defects near the surface is added to the increased gain value at this time, and obtaining a first gain value, and using the first gain value as the gain value for detecting defects near the surface of the shaft hole of the support frame casting this time; S302, by adjusting the gain button of the ultrasonic flaw detector, the artificial defects on the far surface of the ultrasonic comparison test block (8) are detected, so that the wave height of the defect wave reaches 80% of the ultrasonic display, and these gain values are recorded respectively; then, a position with uniform wall thickness is selected in the axial hole (2) of the ultrasonic comparison test block (8) for detection, and the gain button is adjusted to make the bottom wave wave height reach 80% of the observation interface, and then the ultrasonic flaw detector under this gain is placed at the same thickness position of the axial hole of the support frame casting, and the difference in wave height between the two is observed at this time; if the bottom wave on the support frame casting is higher than the bottom wave of the ultrasonic comparison test block (8), the gain is reduced so that the wave height reaches 80% of the observation interface, and the reduced gain is recorded at this time. The gain value is obtained by subtracting the reduced gain value at this time from the maximum gain value previously adjusted on the ultrasonic comparison test block (8) for detecting artificial defects on the far surface, and obtaining a second gain value, and using the second gain value as the gain value for detecting defects on the far surface of the shaft hole of the support frame casting this time; if the bottom wave height on the support frame casting is lower than the bottom wave of the ultrasonic comparison test block (8), the gain is increased so that the wave height reaches 80% of the observation interface, and the increased gain value at this time is recorded, and the maximum gain value previously adjusted on the ultrasonic comparison test block (8) for detecting artificial defects on the far surface is added to the increased gain value at this time, and obtaining a second gain value, and using the second gain value as the gain value for detecting defects on the far surface of the shaft hole of the support frame casting this time.
7. An ultrasonic detection method for the position of the shaft hole of a support frame casting according to claim 6, characterized in that: In step S4, the support frame casting is inspected, including the following steps: S401, adjusting the gain of the ultrasonic flaw detector to the first gain value in step S301, tightly coupling the ultrasonic probe to the detected position of the shaft hole of the support frame casting, scanning the shaft hole of the support frame casting at a speed of no more than 50 mm / s using a longitudinal wave vertical incidence method, detecting the internal metallurgical defects near the surface of the shaft hole, and judging whether there are excessive defects in the detection area by observing the change of its waveform; S402, adjusting the gain of the ultrasonic flaw detector to the second gain value in step S302, tightly coupling the ultrasonic probe to the detected position of the shaft hole of the support frame casting, using the longitudinal wave vertical incidence method to scan the shaft hole of the support frame casting at a speed not exceeding 50 mm / s, detecting the internal metallurgical defects at the far surface of the shaft hole, and judging whether there are excessive defects in the detection area by observing the changes in its waveform.
8. The ultrasonic detection method for the position of the shaft hole of the support frame casting according to claim 1, characterized in that: In the steps S2 to S4, an ultrasonic probe with a frequency of 10 MHz and a size of 0.25 In is selected; the equipment used is an ultrasonic flaw detector with a model of USM33LEMO.
9. The ultrasonic detection method for the position of the shaft hole of the support frame casting according to claim 5, characterized in that: Two artificial defect blind holes are prepared at the root transition fillet positions on both sides of the lower rib plate (6), namely artificial defect A, artificial defect B, artificial defect C and artificial defect D, wherein: Artificial defect A is a blind hole with a hole diameter of φ0.8 mm and a hole depth of 3 mm; The artificial defect B is a blind hole with a hole diameter of φ0.8 mm and a bottom of the hole 3 mm away from the inner wall of the tube body (1); Artificial defect C is a blind hole with a hole diameter of φ1.2mm and a hole depth of 3mm; The artificial defect D is a blind hole with a hole diameter of φ1.2 mm and a bottom distance of 3 mm from the inner wall of the tube body (1); The artificial defect B and the artificial defect D are located on the left side of the lower rib plate (6), and are both 20 mm away from the center of the lower rib plate (6); the distance between the artificial defect B and the inner panel (4) is 30 mm; the distance between the artificial defect D and the inner panel (4) is 55 mm; The artificial defect A and the artificial defect C are located on the right side of the lower rib plate (6); both are 20 mm away from the center of the lower rib plate (6); the distance between the artificial defect A and the inner panel (4) is 30 mm; the distance between the artificial defect C and the inner panel (4) is 55 mm.
10. The ultrasonic detection method for the position of the shaft hole of the support frame casting according to claim 5, characterized in that: An artificial defect blind hole is prepared at the root transition fillet position on both sides of the reinforcing rib (7), respectively, and they are artificial defect E and artificial defect F; an artificial defect blind hole is prepared at the root transition fillet position on both sides of the upper rib plate (5), respectively, and they are artificial defect G and artificial defect H; Artificial defect E is a blind hole with a hole diameter of φ0.8 mm and a hole depth of 3 mm; The artificial defect F is a blind hole with a hole diameter of φ0.8 mm and a bottom of the hole 3 mm away from the inner wall of the tube body (1); The artificial defect G is a blind hole with a hole diameter of φ1.2mm and a hole depth of 3mm; The artificial defect H is a blind hole with a hole diameter of φ1.2 mm and a bottom of the hole 3 mm away from the inner wall of the tube body (1); The artificial defect E is located on the right side of the reinforcing rib (7), and the artificial defect F is located on the left side of the reinforcing rib (7); the artificial defect E and the artificial defect F are respectively 20 mm away from the center of the reinforcing rib (7), and are respectively 20 mm away from the outer panel (3); The artificial defect H is located on the right side of the upper rib plate (5), and the artificial defect G is located on the left side of the upper rib plate (5); The artificial defect H and the artificial defect G are respectively 20 mm away from the center of the upper rib plate (5) and 19 mm away from the outer panel (3).