Al-coated Ag conductive paste and preparation method thereof
Al@Ag conductive paste is prepared by plating silver on the surface of aluminum powder and mixing it with epoxy resin, which solves the problems of poor conductivity and low oxidation resistance, improves the conductivity and oxidation resistance, and is suitable for high-end applications. And reduce costs.
Patent Information
- Application Number
- CN202411242589.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing conductive pastes have poor electrical conductivity and low oxidation resistance, which affects their stability and performance at high temperatures and long-term use.
Magnetically controlled sputtering method is used to plate silver on the surface of aluminum powder, and mix silver-plated aluminum powder with epoxy resin, coupling agent and defoaming agent to prepare Al@Ag conductive paste to improve its conductivity and oxidation resistance. sex.
Improve the conductive properties and oxidation resistance of conductive pastes, making them better in high-end applications such as electromagnetic shielding and anti-static areas, while reducing production costs. It also uses epoxy resins and magnetron sputtering processes to be simple and easy to use. control.
Smart Images

Figure CN119028630A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of slurry preparation, and in particular relates to a preparation method of Al@Ag conductive slurry, and also relates to the Al@Ag conductive slurry. Background Art
[0002] With the development of electronic information, the demand for membrane switches, flexible printed circuits, electromagnetic shielding, solar cells, etc. is growing. Various high-tech electronic products are favored by the public, and higher requirements are also put forward for new electronic products. Conductive paste, as a key raw material in its preparation process, plays a vital role in the development of various fields, and promotes the development of electronic technology products towards miniaturization, lightness, functionality and low cost. Among them, conductive silver paste belongs to the filling conductive paste. The conductivity of the conductive channel mainly depends on the conductive filler. Its performance and content have a vital influence on the performance of silver paste. The structure determines the performance. The size, morphology, surface state and dispersibility of silver powder in organic carriers can directly affect the conductive properties of conductive silver paste. However, the use of silver powder causes a sharp increase in the cost of preparing conductive paste. Therefore, the use of silver-plated aluminum powder as a conductive filler can reduce costs. It is particularly important to develop conductive pastes with lower costs.
[0003] A Chinese patent (application number: 202110516758.0, publication number: CN 113257456 A, publication date: 2021.08.13) discloses a low-cost conductive paste for heterojunction solar cells and a preparation method thereof. The conductive paste includes: flaky silver-coated aluminum powder, spherical silver powder, nano silver powder, resin, curing agent, and additives; flaky silver-coated aluminum powder and spherical silver powder are used. The use of flaky silver-coated aluminum powder is conducive to improving the mesh performance of the conductive paste and reducing the production cost of the conductive paste. The use of flaky silver-coated aluminum powder with spherical silver powder can further improve the mesh performance of the prepared conductive paste. Although it contains silver powder in different forms, flaky silver-coated aluminum powder is the dominant component. The conductivity of aluminum is relatively weaker than that of silver, which may affect the overall conductive performance to a certain extent. Compared with pure silver conductive paste, its conductivity may be lower.
[0004] A Chinese patent (application number: 202111111878.9, publication number: CN 113555145 B, publication date: 2022.03.25) discloses a flexible high temperature resistant conductive paste, including: conductive powder, high heat resistant resin, epoxy resin, amine curing agent, imidazole curing accelerator, amino silicone oil modified epoxy resin, solvent, coupling agent, rheological additive; the conductive powder contains one or more selected from silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, silver-coated aluminum powder and silver-coated glass powder; the cured film of the conductive paste has good flexibility and can be applied to flexible substrates such as PEEK and PI, and the cured film has excellent high temperature resistance. However, in actual applications, its high temperature resistance may be affected by many factors. The difference in thermal expansion coefficients between different components may cause delamination, cracking and other problems at high temperatures, thereby affecting the overall performance of the conductive paste. Moreover, when exposed to high temperature for a long time, the conductive powder may undergo chemical reactions such as oxidation, reducing the conductive performance. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing Al@Ag conductive paste, which solves the problems of poor conductivity and low oxidation resistance of the existing paste.
[0006] Another object of the present invention is to provide the Al@Ag conductive paste.
[0007] The technical solution adopted by the present invention is a method for preparing Al@Ag conductive paste, which is specifically implemented according to the following steps:
[0008] Step 1, pickling, washing and drying the flaky aluminum powder to obtain pretreated aluminum powder;
[0009] Step 2, placing the pretreated aluminum powder on a vacuum chuck, then fixing it on a sample plate of a magnetron sputtering instrument, placing it in a vacuum chamber, maintaining the vacuum chamber in a vacuum, and performing magnetron sputtering to silver-plate the surface of the pretreated aluminum powder;
[0010] Step 3, adding the silver-plated aluminum powder obtained in step 2 into epoxy resin, and then adding a coupling agent and a defoaming agent and stirring, so as to obtain Al@Ag conductive paste.
[0011] The present invention is also characterized in that:
[0012] In step 1, specifically: flaky aluminum powder with a particle size of 3μm to 10μm is placed in dilute H2SO4 for pickling, the pickled aluminum powder is rinsed with deionized water until the pH of the powder aqueous solution is 7, filtered and dried to obtain pretreated aluminum powder.
[0013] In step 2, during magnetron sputtering, the sputtering power is 50-150W, the sputtering gas pressure is 0.3-0.7Pa, the sputtering bias is -40-80V, and the sputtering time is 10-30mins.
[0014] In step 3, the epoxy resin is a glycidyl ether epoxy resin; the coupling agent is a silane coupling agent, and the defoaming agent is a silicone defoaming agent.
[0015] In step 3, the mass ratio of the silver-plated aluminum powder to the epoxy resin is 6-8:2-4; the coupling agent accounts for 0.8-1.2% of the total mass of the silver-plated aluminum powder, the epoxy resin coupling agent and the defoaming agent, and the defoaming agent accounts for 0.9% of the total mass of the silver-plated aluminum powder, the epoxy resin coupling agent and the defoaming agent.
[0016] In step 3, the stirring speed is 300 r / min and the stirring time is 15-25 minutes.
[0017] Another technical solution adopted by the present invention is the Al@Ag conductive paste prepared by the preparation method of the Al@Ag conductive paste.
[0018] The beneficial effects of the present invention are as follows: the conductivity and oxidation resistance of the silver-plated aluminum powder of the present invention make it more advantageous in high-end applications such as electromagnetic shielding and anti-static fields, and the addition of silver does not change the original properties of the aluminum powder, thereby reducing the cost of the conductive slurry; in the silver plating process, the surface of the aluminum powder is silver-plated by a magnetron sputtering method, with a fast deposition speed, uniform coating, simple equipment, and easy control; epoxy resin is selected as the slurry matrix, which has good bonding strength and is green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The volume resistivity diagram of the conductive paste under different parameters in Examples 1-3;
[0020] Figure 2 It is a graph showing the mass change of the conductive paste under different parameters in Examples 1-3. DETAILED DESCRIPTION
[0021] The present invention is described in detail below in conjunction with specific implementation modes and accompanying drawings.
[0022] The preparation method of the Al@Ag conductive paste of the present invention is specifically implemented according to the following steps:
[0023] Step 1, pickling, washing and drying flaky aluminum powder with a particle size of 3 μm to 10 μm to obtain pretreated aluminum powder;
[0024] Specifically, the flake aluminum powder with a purity greater than 98% is placed in dilute H2SO4 for pickling, the pickled aluminum powder is rinsed with deionized water until the pH of the powder aqueous solution is 7, filtered and dried to obtain the pretreated aluminum powder;
[0025] The mass fraction of dilute H2SO4 is 5%, and the pickling time is 30 minutes;
[0026] Step 2, using magnetron sputtering to plate silver on the pretreated aluminum powder;
[0027] The pretreated aluminum powder is placed on a vacuum chuck, then fixed on a sample plate of a magnetron sputtering instrument, placed in a vacuum chamber, and the vacuum chamber is kept vacuum to perform magnetron sputtering to silver plate the surface of the pretreated aluminum powder;
[0028] During magnetron sputtering, the sputtering power is 50-150w, the sputtering gas pressure is 0.3-0.7Pa, the sputtering bias is -40~80V, and the sputtering time is 10-30mins;
[0029] Step 3, adding the silver-plated aluminum powder obtained in step 2 into epoxy resin, then adding a coupling agent and a defoaming agent, stirring at room temperature, and obtaining Al@Ag conductive paste.
[0030] The epoxy resin is a glycidyl ether epoxy resin; the coupling agent is a silane coupling agent, and the defoaming agent is an organic silicon defoaming agent;
[0031] The mass ratio of silver-plated aluminum powder to epoxy resin is 6-8:2-4; the coupling agent accounts for 0.8-1.2% of the total mass (the sum of the mass of silver-plated aluminum powder, epoxy resin coupling agent and defoamer), and the defoamer accounts for 0.9% of the total mass;
[0032] The stirring speed is 300r / min and the stirring time is 15-25mins.
[0033] In the Al@Ag conductive paste of the present invention, the silver-plated aluminum powder improves the conductivity and oxidation resistance of the paste, making it more advantageous in high-end applications such as electromagnetic shielding and antistatic fields, and the addition of silver does not change the original properties of the aluminum powder, thereby reducing the cost of the conductive paste.
[0034] Example 1
[0035] The preparation method of the Al@Ag conductive paste of the present invention is specifically implemented according to the following steps:
[0036] Step 1, 10 g of Al powder with an average particle size of 5 μm and a purity greater than 98% is placed in 50 ml of a dilute sulfuric acid aqueous solution (5 wt%) for pickling for 30 mins, then washed with deionized water until the pH is 7, and the Al powder after filtration is placed in an oven at 80° C. to dry to obtain pretreated Al powder;
[0037] Step 2, placing aluminum powder on a vacuum chuck, then fixing it on a sample plate of a magnetron sputtering instrument, and placing it in a vacuum chamber; evacuating the vacuum chamber of the magnetron sputtering instrument to a vacuum state, introducing argon gas at 20 sccm, inputting a sputtering power of 50 W, a sputtering constant voltage of 0.3, a sputtering bias of -40 V, and a sputtering time of 10 min, and then silver-plating the surface of the aluminum powder;
[0038] Step 3, adding the silver-plated aluminum powder obtained in step 2 to the epoxy resin, then adding a coupling agent and a defoaming agent, stirring at room temperature to obtain a mixed slurry, and then obtaining Al@Ag conductive slurry.
[0039] The epoxy resin selected is glycidyl ether epoxy resin; the coupling agent is silane coupling agent, and the defoaming agent is silicone defoaming agent; the mass ratio of silver-plated aluminum powder to epoxy resin is 6:4; the coupling agent accounts for 0.8% of the total mass, the defoaming agent accounts for 0.9% of the total mass, the stirring speed is 300r / min, and the stirring time is 20mins.
[0040] Example 2
[0041] The preparation method of the Al@Ag conductive paste of the present invention is specifically implemented according to the following steps:
[0042] Step 1: Place 10 g of Al powder with an average particle size of 5 μm and a purity greater than 98% in 50 ml of a dilute sulfuric acid aqueous solution (5 wt%) for pickling for 30 minutes, then wash with deionized water until the pH value is 7, and place the filtered Al powder in an oven at 80°C to dry to obtain pretreated Al powder.
[0043] Step 2, place aluminum powder on a vacuum chuck, then fix it on a sample plate of a magnetron sputtering instrument, and place it in a vacuum chamber; evacuate the vacuum chamber of the magnetron sputtering instrument to a vacuum state, introduce argon gas at 20 sccm, input a sputtering power of 100 W, a sputtering constant voltage of 0.5, a sputtering bias of -60 V, and a sputtering time of 20 min to silver-plate the surface of the aluminum powder.
[0044] Step 3, adding the silver-plated aluminum powder obtained in step 2 to the epoxy resin, then adding a coupling agent and a defoaming agent, stirring at room temperature to obtain a mixed slurry, and then obtaining Al@Ag conductive slurry.
[0045] The epoxy resin selected is glycidyl ether epoxy resin; the coupling agent is silane coupling agent, and the defoaming agent is silicone defoaming agent; the mass ratio of silver-plated aluminum powder to epoxy resin is 7:3; the coupling agent accounts for 1% of the total mass, the defoaming agent accounts for 0.9% of the total mass, the stirring speed is 300r / min, and the stirring time is 15mins.
[0046] Example 3
[0047] The preparation method of the Al@Ag conductive paste of the present invention is specifically implemented according to the following steps:
[0048] Step 1: Place 10 g of Al powder with an average particle size of 5 μm and a purity greater than 98% in 50 ml of a dilute sulfuric acid aqueous solution (5 wt%) for pickling for 30 minutes, then wash with deionized water until the pH value is 7, and place the filtered Al powder in an oven at 80°C to dry to obtain pretreated Al powder.
[0049] Step 2, place the aluminum powder on a vacuum chuck, then fix it on the sample plate of the magnetron sputtering instrument, and place it in a vacuum chamber; evacuate the vacuum chamber of the magnetron sputtering instrument to a vacuum state, introduce 20sccm of argon gas, input a sputtering power of 150w, a sputtering constant voltage of 0.7, a sputtering bias of -80V, and a sputtering time of 30min to silver-plate the surface of the aluminum powder.
[0050] Step 3, adding the silver-plated aluminum powder obtained in step 2 to the epoxy resin, then adding a coupling agent and a defoaming agent, stirring at room temperature to obtain a mixed slurry, and then obtaining Al@Ag conductive slurry.
[0051] The epoxy resin selected is glycidyl ether epoxy resin; the coupling agent is a silane coupling agent, and the defoaming agent is a silicone defoaming agent; the mass ratio of silver-plated aluminum powder to epoxy resin is 8:2; the coupling agent accounts for 1.2% of the total mass, the defoaming agent accounts for 0.9% of the total mass, the stirring speed is 300r / min, and the stirring time is 25mins.
[0052] Figure 1 It is a volume resistivity diagram of the conductive paste under different parameters in Examples 1-3. It can be seen from the figure that the conductive paste of the present invention has excellent conductive properties, and the conductive paste prepared in Example 3 has the best conductive properties. This is because the conductive filler is the only source of the conductive properties of the conductive glue, and the resistivity directly affects the conductive properties of the conductive glue. As the silver content of the conductive filler particles increases, the conductive properties of the conductive glue gradually improve. The conductivity and oxidation resistance of metallic silver are better than those of metallic aluminum. The silver layer coated on the surface of the aluminum powder can improve the antioxidant and conductive properties of the aluminum powder. However, the antioxidant and conductive properties of the conductive powder are different due to the different silver content of the coating. When the silver content is low, the coating is not complete, the silver coating on the surface of the aluminum powder is not dense enough, and there are uncoated parts of the powder, which are prone to oxidation, resulting in a decrease in conductive properties. The conductive network formation inside the conductive paste is not complete, that is, the conductive properties are reduced. When the magnetron sputtering power increases, the silver particles coated on the surface of the aluminum powder are more complete, so the more complete the conductive path, the better the conductive properties, and the lower the resistivity.
[0053] Figure 2It is a graph showing the mass change of the conductive paste under different parameters in Examples 1-3. The mass of the three conductive pastes also increases to a certain extent as the storage time increases under room temperature. This is because the conductive film reacts with the oxygen in the air during storage to generate a small amount of oxide, which causes the mass of the sample to increase. In the early stage of the test, the conductive phase in the conductive paste has a high surface activity and is in a period of easy oxidation and corrosion. It is easy to combine with oxygen in the air to generate oxides and adsorb on the surface. Therefore, the mass increase rate of the conductive paste is relatively fast. As the test cycle increases, more and more oxide films are adsorbed on the surface, which reduces the area and probability of oxygen contact in the air. The oxide film layer also plays a certain role in isolating the conductive phase from oxygen.
Claims
1. A method for preparing Al@Ag conductive paste, characterized in that: Follow the steps below to implement it: Step 1, pickling, washing and drying the flaky aluminum powder to obtain pretreated aluminum powder; Step 2, placing the pretreated aluminum powder on a vacuum chuck, then fixing it on a sample plate of a magnetron sputtering instrument, placing it in a vacuum chamber, maintaining the vacuum chamber in a vacuum, and performing magnetron sputtering to silver-plate the surface of the pretreated aluminum powder; Step 3, adding the silver-plated aluminum powder obtained in step 2 into epoxy resin, and then adding a coupling agent and a defoaming agent and stirring, so as to obtain Al@Ag conductive paste.
2. The method for preparing the Al@Ag conductive paste according to claim 1, characterized in that: In step 1, specifically: flaky aluminum powder with a particle size of 3μm to 10μm is placed in dilute H2SO4 for pickling, the pickled aluminum powder is rinsed with deionized water until the pH of the powder aqueous solution is 7, filtered and dried to obtain pretreated aluminum powder.
3. The method for preparing the Al@Ag conductive paste according to claim 1, characterized in that: In the step 2, during magnetron sputtering, the sputtering power is 50-150W, the sputtering gas pressure is 0.3-0.7Pa, the sputtering bias is -40-80V, and the sputtering time is 10-30mins.
4. The method for preparing the Al@Ag conductive paste according to claim 1, characterized in that: In the step 3, the epoxy resin is a glycidyl ether epoxy resin; the coupling agent is a silane coupling agent, and the defoaming agent is a silicone defoaming agent.
5. The method for preparing the Al@Ag conductive paste according to claim 1, characterized in that: In the step 3, the mass ratio of the silver-plated aluminum powder to the epoxy resin is 6-8:2-4; the coupling agent accounts for 0.8-1.2% of the total mass of the silver-plated aluminum powder, the epoxy resin coupling agent and the defoaming agent, and the defoaming agent accounts for 0.9% of the total mass of the silver-plated aluminum powder, the epoxy resin coupling agent and the defoaming agent.
6. The method for preparing the Al@Ag conductive paste according to claim 1, characterized in that: In step 3, the stirring speed is 300 r / min and the stirring time is 15-25 minutes.
7. The Al@Ag conductive paste prepared by the method for preparing the Al@Ag conductive paste according to any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method for UV light-cured silver-coated nickel conductive slurry
CN105161219A
Method for preparing TixSi1-xC / Ag composite conductive coating
CN109706430A
Preparation method of novel conductive silver adhesive with high heat conductivity coefficient and conductive silver adhesive
CN111518501A
Preparation method of hole-plugging silver paste for interconnection of any layer of multifunctional board and hole plugging silver paste
CN111584154A
Preparation method of low-emissivity color composite pigment
CN115584145A