Preparation process of miniature supercapacitor

By directly coating the electrode material on the surface of the negative electrode column in the supercapacitor, the problems of complex production process and insufficient capacitor performance in the prior art are solved, and more efficient and convenient preparation of micro supercapacitors is achieved, and the capacitor is improved. Lifespan and voltage.

CN119028738AActive Publication Date: 2024-11-26FUJIAN TORCH ELECTRON TECH CO LTD

Patent Information

Application Number
CN202411380480.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-26
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

The existing supercapacitors have problems such as shrinking volume and high manufacturing cost, limited ionic conductivity, poor mechanical strength, low working temperature range, and easy to break in terms of volume reduction, especially supercapacitors using solid electrolytes, and many other defects are present. Small column supercapacitors have low voltage and need to be connected in series to increase costs.

Method used

Using the preparation process of micro supercapacitors, by directly coating the electrode material on the negative electrode column and the inner wall surface of the accommodating cavity, using unique electrode material coating and rolling methods, reducing the process, avoiding the use of conductive gels and other materials, and improving the The contact density between the electrode material and the current collector increases the aging space of the positive electrode material and simplifies the structure.

Benefits of technology

It reduces the internal resistance of the capacitor, improves the service life and voltage, simplifies the process, realizes a more convenient internal series supercapacitor, and reduces the unqualified yield and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028738A_ABST
    Figure CN119028738A_ABST
Patent Text Reader

Abstract

According to the preparation technology of the miniature supercapacitor, the miniature supercapacitor comprises a first monomer unit and a first negative pole unit capable of being connected with the first monomer unit, and the first monomer unit comprises a first shell internally provided with a first containing cavity and a first positive pole arranged in the first containing cavity; the outer wall of the first positive pole is attached to the inner wall of the first accommodating cavity; the first negative pole unit comprises a first negative pole capable of being embedded into the first positive pole, a first diaphragm layer wrapping the peripheral surface of the first negative pole, and a first sealing rubber ring which sleeves the upper end of the first negative pole and is used for sealing the first accommodating cavity; by limiting the structural design of the miniature capacitor, the electrode column and the shell directly serve as the current collector, the contact between the electrode material and the current collector is more compact through unique electrode material coating, rolling and rolling modes, the material is uniform, the structure is firm, the process is simple, and the internal resistance of the capacitor is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of supercapacitor preparation, and in particular relates to a preparation process of a micro supercapacitor. Background Art

[0002] As an emerging advanced energy storage device, supercapacitors have both the high power characteristics of traditional capacitors and the high energy characteristics of batteries. Due to its unique high specific power, large current discharge capability, ultra-long temperature and wide range characteristics, and high reliability and green environmental protection characteristics such as no discharge voltage platform, it has been widely used and developed in many fields such as electricity, transportation, communications, energy, aviation, etc.

[0003] The existing supercapacitors are greatly limited in size due to the structure, manufacturing process, and manufacturing equipment. Especially for the mainstream supercapacitors on the market that use organic electrolytes as carriers, for supercapacitors that use solid electrolytes as carriers, due to their relatively immature technology, there are many defects such as high manufacturing cost, limited ionic conductivity, poor mechanical strength, low operating temperature range, limited contact area resulting in low specific capacity, easy rupture and capacitor short circuit. These are obstacles to the use of solid electrolytes to prepare supercapacitors. In comparison, the supercapacitor system using organic electrolytes as carriers has undergone decades of research and development and improvement, with mature technology, stable performance and high cost performance. At the same time, the existing small column supercapacitors generally use a jack-type lead-out method, which has its limitations for the design of user circuit boards, and the use voltage of a single supercapacitor is low. It is usually necessary to connect them in series after the supercapacitor unit is prepared to increase the rated voltage of the module supercapacitor. This method adds multiple processes such as welding, cutting feet, and secondary packaging, increases the defective rate and labor in the manufacturing process, and increases the cost, which needs further improvement. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a preparation process for a micro supercapacitor.

[0005] The present invention adopts the following technical solution: A preparation process of a micro supercapacitor, the micro supercapacitor comprising a first monomer unit and a first negative electrode column unit connectable to the first monomer unit, The first monomer unit comprises a first housing having a first accommodating cavity formed therein and a first positive electrode column disposed in the first accommodating cavity, wherein an outer wall of the first positive electrode column is in contact with an inner wall of the first accommodating cavity; The first negative electrode column unit comprises a first negative electrode column that can be embedded in the first positive electrode column, a first diaphragm layer wrapped around the outer circumference of the first negative electrode column, and a first sealing rubber ring sleeved on the upper end of the first negative electrode column for sealing the first accommodating cavity, wherein a first positioning hole for embedding the first negative electrode column is formed inside the first positive electrode column; The preparation process comprises the following steps: Step 1: insert the first negative electrode column into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the first negative electrode column, dry and shape to form a first diaphragm layer, and then fix the first sealing rubber ring on the upper end of the first negative electrode column to obtain a first negative electrode column unit; Step 2: Lay the first housing flat, plug the first accommodating cavity with a plug having a through hole formed therein, inject the positive electrode slurry into the first accommodating cavity using a syringe, rotate the first housing around its axis, evenly coat the positive electrode slurry on the inner wall of the first accommodating cavity, adhere and shape it, remove the plug, and use a positive electrode rolling device to roll and shape the positive electrode slurry, so that the first positive electrode column is formed inside the first accommodating cavity to obtain a first monomer unit; Step three, injecting electrolyte into the first shell, then inserting the first negative electrode column of the first negative electrode column unit into the first positioning hole of the first positive electrode column, and engaging the first sealing rubber ring with the inner wall of the first accommodating cavity to obtain the micro supercapacitor.

[0006] Furthermore, the first negative electrode column includes a first supporting portion that can be supported at the upper end of the first outer shell, a first extension section that is arranged at the lower end of the first supporting portion and extends downward, a first connecting column that is arranged at the lower end of the first extension section and extends downward and can be embedded in the first positioning hole, and a first negative electrode column body wrapped around the outer periphery of the first connecting column, the first sealing rubber ring is arranged around the outer periphery of the first extension section, and the first diaphragm layer is wrapped around the outer periphery of the first negative electrode column.

[0007] Furthermore, when preparing the first negative electrode column, the first connecting column is inserted into the negative electrode slurry to make the negative electrode slurry adhere to the first connecting column, and the negative electrode slurry is firmly adhered to the outer periphery of the first connecting column through rotation, drying and rolling to form a first negative electrode column.

[0008] Furthermore, the first sealing rubber ring includes a first main body section that can be embedded in the first accommodating cavity and a first limiting section arranged at the upper end of the first main body section and can be supported at the upper end of the first accommodating cavity, and the bottom surface of the first supporting portion is in contact with the top surface of the first limiting section.

[0009] Furthermore, the positive electrode rolling device includes a fixed column that can be docked with the first shell and a rolling and shaping column that can be movably arranged in the fixed column, the fixed column is formed with a movable cavity for the rolling and shaping column to move back and forth, and a shaping portion is formed at the front end of the rolling and shaping column, and the diameter of the shaping portion is the same as the diameter of the first positioning hole. When the first positive electrode column is prepared, the fixed column is docked with the first shell, and the rolling and shaping column moves in a direction close to the positive electrode slurry so that the shaping portion extends into the positive electrode slurry. Through the repeated back and forth movement of the rolling and shaping column, the positive electrode slurry is solidified and formed in the accommodating cavity to obtain the first positive electrode column.

[0010] Furthermore, it also includes a negative electrode lead-out terminal arranged at the upper end of the first negative electrode column and a positive electrode lead-out terminal arranged at the bottom of the first shell.

[0011] Furthermore, the negative electrode lead-out terminal includes a negative electrode positioning section arranged at the upper end of the first negative electrode column and a negative electrode connecting section extending outward from the side of the negative electrode positioning section, and the positive electrode lead-out terminal includes a positive electrode positioning section arranged at the bottom of the first shell and a positive electrode connecting section extending outward from the side of the positive electrode positioning section. The contact surfaces of the negative electrode connecting section, the positive electrode connecting section and the circuit board are all provided with a tin plating layer. In step three, after the first sealing rubber ring is engaged with the inner wall of the accommodating cavity, the contact surfaces of the negative electrode connecting section, the positive electrode connecting section and the circuit board are tin-plated to form a tin plating layer to obtain the micro supercapacitor.

[0012] A preparation process of a micro supercapacitor, the micro supercapacitor comprising a first monomer unit, a first negative electrode column unit and a plurality of second monomer units spliced ​​between the first monomer unit and the first negative electrode column unit, The first monomer unit comprises a first housing having a first accommodating cavity formed therein and a first positive electrode column disposed in the first accommodating cavity, wherein an outer wall of the first positive electrode column is in contact with an inner wall of the first accommodating cavity; The first negative electrode column unit comprises a first negative electrode column that can be embedded in the first positive electrode column, a first diaphragm layer wrapped around the outer circumference of the first negative electrode column, and a first sealing rubber ring sleeved on the upper end of the first negative electrode column for sealing the first accommodating cavity, wherein a first positioning hole for embedding the first negative electrode column is formed inside the first positive electrode column; The second monomer unit includes a second housing with a second accommodating cavity formed therein, a second positive electrode column disposed in the second accommodating cavity, a second negative electrode column disposed at the bottom of the second housing and extending downwardly and capable of being embedded in the first positioning hole or the second positive electrode column, a second diaphragm layer wrapped around the outer circumference of the second negative electrode column, and a second sealing rubber ring sleeved on the upper end of the second negative electrode column for sealing the second accommodating cavity or the upper end of the first accommodating cavity, wherein a second positioning hole for the first negative electrode column or the second negative electrode column to be embedded is formed inside the second positive electrode column; The preparation process comprises the following steps: Step 1: insert the first negative electrode column into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the first negative electrode column, dry and shape to form a first diaphragm layer, and then fix the first sealing rubber ring on the upper end of the first negative electrode column to obtain a first negative electrode column unit; Step 2: insert the second negative electrode column into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the second negative electrode column, dry and shape to form a second diaphragm layer, and then fix the second sealing rubber ring on the upper end of the second negative electrode column; Step 3, lay the first housing and the second housing flat, plug the first accommodating cavity and the second accommodating cavity respectively with plugs with through holes formed therein, then use a syringe to inject positive electrode slurry into the first accommodating cavity and the second accommodating cavity respectively, rotate the first housing and the second housing around their axes respectively, so that the positive electrode slurry is evenly coated on the inner wall of the accommodating cavity and adhered to shape, remove the plugs, and use a positive electrode rolling device to roll and shape the positive electrode slurry, so that the first positive electrode column or the second positive electrode column is formed inside the first accommodating cavity and the second accommodating cavity respectively, to obtain a first monomer unit and a second monomer unit; Step 4, injecting the electrolyte into the first shell and the second shell, and then inserting the second negative electrode column of the second monomer unit into the first positioning hole of the first positive electrode column, so that the second sealing rubber ring on the second negative electrode column is engaged in the first accommodating cavity, and continuing to stack the required number of second monomer units on the second monomer unit. During the stacking process, the second negative electrode column of the second monomer unit is inserted into the second positioning hole of the second positive electrode column, so that the second sealing rubber ring is engaged with the inner wall of the second accommodating cavity of the second shell at the lower end; then the first negative electrode column of the first negative electrode column unit is inserted into the first positioning hole of the second positive electrode column at the upper end, so that the first sealing rubber ring is engaged with the inner wall of the second accommodating cavity, and the micro supercapacitor is obtained.

[0013] Furthermore, the second negative electrode column includes a second extension section extending downward from the bottom of the second outer shell, a second connecting column arranged at the lower end of the second extension section and extending downward, and a second negative electrode column wrapped around the outer periphery of the second connecting column, and the second sealing rubber ring is arranged around the outer periphery of the second extension section.

[0014] Furthermore, the second extension section, the second connecting column and the second shell are integrally formed.

[0015] From the above description of the present invention, it can be seen that compared with the prior art, the beneficial effects of the present invention are as follows: the present application simplifies the coating process, slitting, punching, winding or patching process after the ingredients are mixed in the prior art supercapacitor preparation process by limiting the structural design of the microcapacitor, and directly coats the electrode material on the negative electrode column and the inner wall surface of the accommodating cavity, thereby saving a large number of processes and working hours. At the same time, conductive gel, aluminum foil, copper foil, adapter and other materials are no longer used, but the electrode column and the shell are directly used as the current collector, and the electrode material and the current collector are directly connected by a unique electrode material coating, rolling and rolling method. The contact is tighter, the material is uniform, the structure is firm, and the process is simple, which greatly reduces the internal resistance of the capacitor. Among them, because the positive electrode is at a high potential, it is easier to produce chemical side reactions, which accelerates the aging of the material. Therefore, the positive electrode slurry is coated on the inner wall of the shell with a larger area, so that the positive electrode column and the negative electrode column are wrapped in a scattered shape, and more material aging and loss space is reserved for the positive electrode column, which greatly improves the service life of the capacitor. At the same time, the structure is simplified, and it is easy to prepare a sealed electrolyte micro-supercapacitor with solid or liquid selection, realizing a more convenient internal series supercapacitor and increasing the use voltage of the supercapacitor. In addition, by setting a negative lead-out terminal at the upper end of the first negative pole and a positive lead-out terminal at the bottom of the first shell, and by adjusting the lead-out terminal form, it is easier to choose a plug-in type or a patch type installation method for the supercapacitor. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a structural schematic diagram of the first embodiment; Figure 2 is a structural cross-sectional view of the first embodiment; Figure 3 It is an exploded schematic diagram of the first embodiment; Figure 4 is a structural schematic diagram of a second embodiment; Figure 5 is a structural cross-sectional view of a second embodiment; Figure 6 is a schematic structural diagram of the second monomer unit; Figure 7 is a schematic structural diagram of a third embodiment; Figure 8 is a structural cross-sectional view of a third embodiment; Fig. 9 This is a flow chart of the preparation of a micro supercapacitor according to the first embodiment; In the figure, 1-first monomer unit, 2-first negative electrode column unit, 3-second monomer unit, 4-negative electrode lead-out terminal, 5-positive electrode lead-out terminal, 6-positive electrode rolling device, 11-first shell, 111-first accommodating cavity, 12-first positive electrode column, 121-first positioning hole, 21-first negative electrode column, 211-first supporting portion, 212-first extension section, 213-first connecting column, 214-first negative electrode column, 22-first diaphragm layer, 23-first sealing rubber ring, 231-first main body section, 232-first limiting section, 31-second outer shell, 311-second accommodating cavity, 32-second positive pole, 321-second positioning hole, 33-second negative pole, 331-second extension section, 332-second connecting column, 333-second negative electrode column, 34-second diaphragm layer, 35-second sealing rubber ring, 41-negative pole positioning section, 42-negative pole connecting section, 51-positive pole positioning section, 52-positive pole connecting section, 61-fixed column, 62-rolling shaping column, 63-moving cavity, 64-shaping part. DETAILED DESCRIPTION

[0017] The present invention is further described below through specific implementation modes.

[0018] Reference Figures 1 to 3 As shown, the first embodiment of the micro supercapacitor includes a first monomer unit 1 and a first negative electrode column unit 2 connected to the first monomer unit 1 .

[0019] The first monomer unit 1 includes a first housing 11 with a first accommodating cavity 111 formed therein and a first positive electrode column 12 disposed in the first accommodating cavity 111 . Specifically, the outer wall of the first positive electrode column 12 is in contact with the inner wall of the first accommodating cavity 111 .

[0020] The first negative electrode column unit 2 includes a first negative electrode column 21 that can be embedded in the first positive electrode column 12, a first diaphragm layer 22 wrapped around the outer circumference of the first negative electrode column 21, and a first sealing rubber ring 23 sleeved on the upper end of the first negative electrode column 21 for sealing the first accommodating cavity 111. Correspondingly, a first positioning hole 121 for embedding the first negative electrode column 21 is formed inside the first positive electrode column 12; specifically, the height of the first diaphragm layer 22 is consistent with the height of the first positive electrode column 12.

[0021] The first negative electrode column 21 includes a first supporting portion 211 that can be supported on the upper end of the first shell 11, a first extension section 212 that is arranged at the lower end of the first supporting portion 211 and extends downward, a first connecting column 213 that is arranged at the lower end of the first extension section 212 and extends downward and can be embedded in the first positioning hole 121, and a first negative electrode column 214 wrapped around the outer periphery of the first connecting column 213, wherein the first sealing rubber ring 23 is sleeved on the outer periphery of the first extension section 212, and the first diaphragm layer 22 is wrapped around the outer periphery of the first negative electrode column 214; specifically, the diameter of the first connecting column 213 is smaller than the diameter of the first extension section 212; further, the first supporting portion 211, the first extension section 212 and the first connecting column 213 are integrally formed.

[0022] The first sealing rubber ring 23 includes a first main section 231 that can be embedded in the first accommodating cavity 111 and a first limiting section 232 that is arranged at the upper end of the first main section 231 and can be supported at the upper end of the first accommodating cavity 111. When the first sealing rubber ring 23 is installed, the bottom surface of the first supporting portion 211 contacts the top surface of the first limiting section 232; specifically, after the first sealing rubber ring 23 is installed, there is a certain distance between the bottom surface of the first main section 231 and the top surface of the first diaphragm layer 22 or the first positive electrode column 12, so that after the first sealing rubber ring 23 is installed, there is a space between the first diaphragm layer 22 and the first positive electrode column 12. This space makes the internal air pressure of the capacitor more stable, thereby avoiding the reduction of electrical performance due to the increase of internal air pressure of the capacitor caused by decomposition of the electrolyte and gas production.

[0023] The preparation process specifically comprises the following steps: Step 1: insert the first connecting column 213 into the negative electrode slurry, so that the negative electrode slurry adheres to the first connecting column 213, and the negative electrode slurry is firmly adhered to the outer periphery of the first connecting column 213 by rotation, drying, and rolling to form a first negative electrode column 214, thereby obtaining a first negative electrode column 21; Step 2: insert the first negative electrode column 21 into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the first negative electrode column 21, dry and shape to form a first diaphragm layer 22, and then fix the first sealing rubber ring 23 on the upper end of the first negative electrode column 21 to obtain the first negative electrode column unit 2; Step 3: Lay the first housing 11 flat, plug the first accommodating cavity 111 with a plug having a through hole formed therein, then inject the positive electrode slurry into the first accommodating cavity 111 using a syringe, rotate the first housing 11 around its axis at a limited temperature, and use centrifugal action to evenly coat the positive electrode slurry on the inner wall of the first accommodating cavity 111, adhere and shape it, remove the plug, and use the positive electrode rolling device 6 to roll and shape the positive electrode slurry, so that the first positive electrode column 12 is formed inside the first accommodating cavity 111, thereby obtaining the first monomer unit 1; Step 4: inject the electrolyte into the first shell 11, then insert the first negative electrode column 21 of the first negative electrode column unit 2 into the first positioning hole 121 of the first positive electrode column 12, and the first sealing rubber ring 23 is engaged with the inner wall of the first accommodating cavity 111 to obtain the above-mentioned micro supercapacitor.

[0024] Among them, negative electrode slurry, cellulose pulp, and positive electrode slurry are commonly used components in the field of supercapacitor preparation. Since they are not the invention points of this application, the raw material composition of their components will not be further described here, and the specific parameters of the corresponding drying and shaping processes also refer to the existing processes; specifically, the thickness of the negative electrode column and the positive electrode column determines the size of the micro supercapacitor, and the fluidity of the slurry can be increased or decreased by adjusting the solid content of the electrode slurry to adjust the thickness of the positive electrode and the negative electrode after molding. When the fluidity is high, the thinner the thickness of the electrode column attached to the connecting column and the inner wall of the accommodating cavity, the smaller the size of the capacitor can be. Among them, the thinnest electrode column can reach the nanometer-level thickness of the raw material particles, and the capacitor diameter can reach 100um or less.

[0025] Reference Fig. 9 As shown, the positive electrode rolling device 6 includes a fixed column 61 that can be docked with the first shell 11 and a rolling and shaping column 62 that can be movably arranged in the fixed column 61, wherein the fixed column 61 is formed with a movable cavity 63 for the rolling and shaping column 62 to move back and forth, and a shaping portion 64 is formed at the front end of the rolling and shaping column 62, and the diameter of the shaping portion 64 is the same as the diameter of the first positioning hole 121; specifically, when the first positive electrode column 12 is prepared, the fixed column 61 is docked with the first shell 11, and the rolling and shaping column 62 moves in a direction close to the positive electrode slurry so that the shaping portion 64 extends into the positive electrode slurry, and the positive electrode slurry is solidified and formed in the first accommodating cavity 111 through the repeated back and forth movement of the rolling and shaping column 62, so as to obtain the first positive electrode column 12.

[0026] Reference Figures 4 to 6 As shown, the second embodiment of the micro supercapacitor includes a first monomer unit 1 , a first negative electrode column unit 2 , and a plurality of second monomer units 3 spliced ​​between the first monomer unit 1 and the first negative electrode column unit 2 .

[0027] The structures of the first monomer unit 1 and the first negative electrode column unit 2 are the same as those of the first monomer unit and the first negative electrode column unit in the first embodiment.

[0028] The second monomer unit 2 includes a second outer shell 31 with a second accommodating cavity 311 formed therein, a second positive electrode column 32 arranged in the second accommodating cavity 311, a second negative electrode column 33 arranged at the bottom of the second outer shell 31 and extending downwardly and can be embedded in the first positioning hole 121 or the second positive electrode column 32, a second diaphragm layer 34 wrapped around the outer circumference of the second negative electrode column 33, and a second sealing rubber ring 35 sleeved on the upper end of the second negative electrode column 33 for sealing the second accommodating cavity 311 or the upper end of the first accommodating cavity 111, wherein a second positioning hole 321 for the first negative electrode column 21 or the second negative electrode column 33 to be embedded is formed inside the second positive electrode column 32.

[0029] The second negative electrode column 33 includes a second extension section 331 extending downward from the bottom of the second outer shell 31, a second connecting column 332 extending downward from the lower end of the second extension section 331, and a second negative electrode column 333 wrapped around the outer periphery of the second connecting column 332, wherein the second sealing rubber ring 35 is sleeved on the outer periphery of the second extension section 331, and the structure is the same as that of the first sealing rubber ring 23; specifically, the second extension section 331, the second connecting column 332 and the second outer shell 31 are integrally formed.

[0030] The preparation process specifically comprises the following steps: Step 1: insert the first connecting column 213 into the negative electrode slurry, so that the negative electrode slurry adheres to the first connecting column 213, and the negative electrode slurry is firmly adhered to the outer periphery of the first connecting column 213 by rotation, drying, and rolling to form a first negative electrode column 214, thereby obtaining a first negative electrode column 21; Step 2: insert the second connecting column 332 into the negative electrode slurry, so that the negative electrode slurry adheres to the second connecting column 332, and the negative electrode slurry is firmly adhered to the outer periphery of the second connecting column 332 by rotation, drying, and rolling to form a second negative electrode column 333, thereby obtaining a second negative electrode column 33; Step 3: insert the first negative electrode column 21 into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the first negative electrode column, dry and shape to form a first diaphragm layer 22, and then fix the first sealing rubber ring 23 on the upper end of the first negative electrode column 21 to obtain the first negative electrode column unit 2; Step 4: insert the second negative electrode column 33 into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the second negative electrode column 33, dry and shape to form a second diaphragm layer 34, and then fix the second sealing rubber ring 35 on the upper end of the second negative electrode column 33; Step 5, the first housing 11 and the second housing 31 are laid flat, and the first accommodating cavity 111 and the second accommodating cavity 311 are blocked with plugs having through holes therein, and then the positive electrode slurry is injected into the first accommodating cavity 111 and the second accommodating cavity 311 respectively using a syringe, and the first housing 11 and the second housing 31 are rotated around their axes at a limited temperature, and the positive electrode slurry is evenly coated on the inner wall of the accommodating cavity by centrifugal action, and adhered and shaped, the plugs are removed, and the positive electrode slurry is rolled and shaped by a positive electrode rolling device, so that the first positive electrode column 12 or the second positive electrode column 32 is formed in the first accommodating cavity 111 and the second accommodating cavity 311 respectively, to obtain the first monomer unit 1 and the second monomer unit 3; Step six, injecting the electrolyte into the first shell 11 and the second shell 31, and then inserting the second negative electrode column 33 of the second monomer unit 3 into the first positioning hole 121 of the first positive electrode column 12, so that the second sealing rubber ring 35 on the second negative electrode column 33 is engaged in the first accommodating cavity 111, and continue to stack the required number of second monomer units 3 on the second monomer unit 3. During the stacking process, the second negative electrode column 33 of the second monomer unit 3 is inserted into the second positioning hole 321 of the second positive electrode column 32, so that the second sealing rubber ring 35 is engaged with the inner wall of the second accommodating cavity 311 of the second shell 31 located at the lower end; then inserting the first negative electrode column 21 of the first negative electrode column unit 2 into the second positioning hole 321 of the second positive electrode column 32 located at the upper end, so that the first sealing rubber ring 23 is engaged with the inner wall of the second accommodating cavity 311, and the above-mentioned micro supercapacitor is obtained.

[0031] Reference Figures 7 and 8 As shown, the third embodiment of the micro supercapacitor includes a first monomer unit 1, a first negative electrode column unit 2 connected to the first monomer unit 1, a negative electrode lead-out terminal 4 arranged at the upper end of the first negative electrode column unit 2, and a positive electrode lead-out terminal 5 arranged at the bottom of the first monomer unit 1.

[0032] The structures of the first monomer unit 1 and the first negative electrode column unit 2 are the same as those of the first monomer unit and the first negative electrode column unit in the first embodiment.

[0033] The negative electrode lead-out terminal 4 includes a negative electrode positioning section 41 arranged at the upper end of the first negative electrode column 21 and a negative electrode connecting section 42 extending outward from the side of the negative electrode positioning section 41. Specifically, the negative electrode lead-out terminal 4, the first supporting portion 211, the first extending section 212 and the first connecting column 213 are integrally formed.

[0034] The positive electrode lead-out terminal 5 includes a positive electrode positioning segment 51 disposed at the bottom of the first housing 11 and a positive electrode connecting segment 52 extending outward from the side of the positive electrode positioning segment 51 . Specifically, the positive electrode lead-out terminal 5 is integrally formed with the first housing 11 .

[0035] The preparation process specifically comprises the following steps: Step 1: insert the first connecting column 213 into the negative electrode slurry, so that the negative electrode slurry adheres to the first connecting column 213, and the negative electrode slurry is firmly adhered to the outer periphery of the first connecting column 213 by rotation, drying, and rolling to form a first negative electrode column 214, thereby obtaining a first negative electrode column 21; Step 2: insert the first negative electrode column 21 into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the first negative electrode column 21, dry and shape to form a first diaphragm layer 22, and then fix the first sealing rubber ring 23 on the upper end of the first negative electrode column 21 to obtain the first negative electrode column unit 2; Step 3, lay the first housing 1 flat, plug the first accommodating cavity 111 with a plug having a through hole formed therein, then inject the positive electrode slurry into the first accommodating cavity 111 using a syringe, rotate the first housing 11 around its axis at a limited temperature, use centrifugal action to evenly coat the positive electrode slurry on the inner wall of the first accommodating cavity 111, adhere and shape it, remove the plug, and use the positive electrode rolling device 6 to roll and shape the positive electrode slurry, so that the first positive electrode column 12 is formed inside the first accommodating cavity 111, and the first monomer unit 1 is obtained; Step 4, injecting the electrolyte into the first shell 11, and then inserting the first negative electrode column 21 of the first negative electrode column unit 2 into the first positioning hole 121 of the first positive electrode column 12, the first sealing rubber ring 23 is engaged with the inner wall of the first accommodating cavity 111, and then tinning is performed on the contact surface between the negative electrode connecting section 42, the positive electrode connecting section 52 and the circuit board to form a tinned layer to obtain the above-mentioned micro supercapacitor.

[0036] By arranging the negative electrode lead-out terminal 4 at the upper end of the first negative electrode column 21 and arranging the positive electrode lead-out terminal 5 at the bottom of the first shell 11, and adjusting the lead-out terminal form, it is more convenient to select the supercapacitor plug-in type or patch type installation method.

[0037] The present application simplifies the coating process, slitting, punching, winding or patching after the ingredients are mixed in the prior art supercapacitor preparation process by limiting the structural design of the microcapacitor, and directly coats the electrode material on the negative electrode column and the inner wall surface of the accommodating cavity, thereby saving a large number of processes and working hours. At the same time, conductive gel, aluminum foil, copper foil, adapter and other materials are no longer used, but the electrode column and the shell are directly used as the current collector. Through the unique electrode material coating, rolling and rolling methods, the contact between the electrode material and the current collector is made tighter, the material is uniform, the structure is firm, and the process is simple, which greatly reduces the internal resistance of the capacitor; among them, because the positive electrode is at a high potential, it is easier to produce chemical side reactions, which accelerates the aging of the material. Therefore, the positive electrode slurry is coated on the inner wall of the shell with a larger area, so that the positive electrode column and the negative electrode column are wrapped in a scattered shape, and more material aging and loss space is reserved for the positive electrode column, which greatly improves the service life of the capacitor. At the same time, the structure is simplified, and it is easy to prepare a sealed micro-supercapacitor with solid or liquid selectable electrolyte, so as to achieve a more convenient internal series supercapacitor and increase the use voltage of the supercapacitor.

[0038] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. That is, equivalent changes and modifications made according to the application scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A preparation process of a micro supercapacitor, characterized in that: The micro supercapacitor comprises a first monomer unit and a first negative electrode column unit connectable to the first monomer unit. The first monomer unit comprises a first housing having a first accommodating cavity formed therein and a first positive electrode column disposed in the first accommodating cavity, wherein an outer wall of the first positive electrode column is in contact with an inner wall of the first accommodating cavity; The first negative electrode column unit comprises a first negative electrode column that can be embedded in the first positive electrode column, a first diaphragm layer wrapped around the outer circumference of the first negative electrode column, and a first sealing rubber ring sleeved on the upper end of the first negative electrode column for sealing the first accommodating cavity, wherein a first positioning hole for embedding the first negative electrode column is formed inside the first positive electrode column; The preparation process comprises the following steps: Step 1: insert the first negative electrode column into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the first negative electrode column, dry and shape to form a first diaphragm layer, and then fix the first sealing rubber ring on the upper end of the first negative electrode column to obtain a first negative electrode column unit; Step 2: Lay the first housing flat, plug the first accommodating cavity with a plug having a through hole formed therein, inject the positive electrode slurry into the first accommodating cavity using a syringe, rotate the first housing around its axis, evenly coat the positive electrode slurry on the inner wall of the first accommodating cavity, adhere and shape it, remove the plug, and use a positive electrode rolling device to roll and shape the positive electrode slurry, so that the first positive electrode column is formed inside the first accommodating cavity to obtain a first monomer unit; Step three, injecting electrolyte into the first shell, then inserting the first negative electrode column of the first negative electrode column unit into the first positioning hole of the first positive electrode column, and engaging the first sealing rubber ring with the inner wall of the first accommodating cavity to obtain the micro supercapacitor.

2. The preparation process of a micro supercapacitor according to claim 1, characterized in that: The first negative electrode column includes a first supporting portion that can be supported at the upper end of the first outer shell, a first extending section that is arranged at the lower end of the first supporting portion and extends downward, a first connecting column that is arranged at the lower end of the first extending section and extends downward and can be embedded in the first positioning hole, and a first negative electrode column body wrapped around the outer periphery of the first connecting column, the first sealing rubber ring is arranged on the outer periphery of the first extending section, and the first diaphragm layer is wrapped around the outer periphery of the first negative electrode column.

3. The preparation process of a micro supercapacitor according to claim 2, characterized in that: When preparing the first negative electrode column, the first connecting column is inserted into the negative electrode slurry to make the negative electrode slurry adhere to the first connecting column. After rotating, drying and rolling, the negative electrode slurry is firmly adhered to the periphery of the first connecting column to form a first negative electrode column.

4. The preparation process of a micro supercapacitor according to claim 2, characterized in that: The first sealing rubber ring includes a first main body section that can be embedded in the first accommodating cavity and a first limiting section that is arranged at the upper end of the first main body section and can be supported at the upper end of the first accommodating cavity, and the bottom surface of the first supporting portion contacts the top surface of the first limiting section.

5. The preparation process of a micro supercapacitor according to claim 1, characterized in that: The positive electrode rolling device includes a fixed column that can be docked with the first shell and a rolling and shaping column that can be movably arranged in the fixed column. The fixed column is formed with a moving cavity for the rolling and shaping column to move back and forth. The front end of the rolling and shaping column is formed with a shaping portion. The diameter of the shaping portion is the same as the diameter of the first positioning hole. When the first positive electrode column is prepared, the fixed column is docked with the first shell, and the rolling and shaping column moves in a direction close to the positive electrode slurry so that the shaping portion extends into the positive electrode slurry. Through the repeated back and forth movement of the rolling and shaping column, the positive electrode slurry is solidified and formed in the accommodating cavity to obtain the first positive electrode column.

6. The preparation process of a micro supercapacitor according to claim 1, characterized in that: It also includes a negative electrode lead-out terminal arranged at the upper end of the first negative electrode column and a positive electrode lead-out terminal arranged at the bottom of the first shell.

7. The process for preparing a micro supercapacitor according to claim 6, characterized in that: The negative electrode lead-out terminal includes a negative electrode positioning section arranged at the upper end of the first negative electrode column and a negative electrode connecting section extending outward from the side of the negative electrode positioning section, and the positive electrode lead-out terminal includes a positive electrode positioning section arranged at the bottom of the first shell and a positive electrode connecting section extending outward from the side of the positive electrode positioning section. The contact surfaces of the negative electrode connecting section, the positive electrode connecting section and the circuit board are all provided with a tin-plated layer. In step three, after the first sealing rubber ring is engaged with the inner wall of the accommodating cavity, tin is plated on the contact surfaces of the negative electrode connecting section, the positive electrode connecting section and the circuit board to form a tin-plated layer, thereby obtaining the micro supercapacitor.

8. A process for preparing a micro supercapacitor, characterized in that: The micro supercapacitor comprises a first monomer unit, a first negative electrode column unit and a plurality of second monomer units spliced ​​between the first monomer unit and the first negative electrode column unit. The first monomer unit comprises a first housing having a first accommodating cavity formed therein and a first positive electrode column disposed in the first accommodating cavity, wherein an outer wall of the first positive electrode column is in contact with an inner wall of the first accommodating cavity; The first negative electrode column unit comprises a first negative electrode column that can be embedded in the first positive electrode column, a first diaphragm layer wrapped around the outer circumference of the first negative electrode column, and a first sealing rubber ring sleeved on the upper end of the first negative electrode column for sealing the first accommodating cavity, wherein a first positioning hole for embedding the first negative electrode column is formed inside the first positive electrode column; The second monomer unit includes a second housing with a second accommodating cavity formed therein, a second positive electrode column disposed in the second accommodating cavity, a second negative electrode column disposed at the bottom of the second housing and extending downwardly and capable of being embedded in the first positioning hole or the second positive electrode column, a second diaphragm layer wrapped around the outer circumference of the second negative electrode column, and a second sealing rubber ring sleeved on the upper end of the second negative electrode column for sealing the second accommodating cavity or the upper end of the first accommodating cavity, wherein a second positioning hole for the first negative electrode column or the second negative electrode column to be embedded is formed inside the second positive electrode column; The preparation process comprises the following steps: Step 1: insert the first negative electrode column into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the first negative electrode column, dry and shape to form a first diaphragm layer, and then fix the first sealing rubber ring on the upper end of the first negative electrode column to obtain a first negative electrode column unit; Step 2: insert the second negative electrode column into the prepared cellulose pulp, make the cellulose pulp evenly adhere to the surface of the second negative electrode column, dry and shape to form a second diaphragm layer, and then fix the second sealing rubber ring on the upper end of the second negative electrode column; Step 3, lay the first housing and the second housing flat, plug the first accommodating cavity and the second accommodating cavity respectively with plugs with through holes formed therein, then use a syringe to inject positive electrode slurry into the first accommodating cavity and the second accommodating cavity respectively, rotate the first housing and the second housing around their axes respectively, so that the positive electrode slurry is evenly coated on the inner wall of the accommodating cavity and adhered to shape, remove the plugs, and use a positive electrode rolling device to roll and shape the positive electrode slurry, so that the first positive electrode column or the second positive electrode column is formed inside the first accommodating cavity and the second accommodating cavity respectively, to obtain a first monomer unit and a second monomer unit; Step 4, injecting the electrolyte into the first shell and the second shell, and then inserting the second negative electrode column of the second monomer unit into the first positioning hole of the first positive electrode column, so that the second sealing rubber ring on the second negative electrode column is engaged in the first accommodating cavity, and continuing to stack the required number of second monomer units on the second monomer unit. During the stacking process, the second negative electrode column of the second monomer unit is inserted into the second positioning hole of the second positive electrode column, so that the second sealing rubber ring is engaged with the inner wall of the second accommodating cavity of the second shell at the lower end; then the first negative electrode column of the first negative electrode column unit is inserted into the first positioning hole of the second positive electrode column at the upper end, so that the first sealing rubber ring is engaged with the inner wall of the second accommodating cavity, and the micro supercapacitor is obtained.

9. The process for preparing a micro supercapacitor according to claim 8, characterized in that: The second negative electrode column includes a second extension section extending downward from the bottom of the second outer shell, a second connecting column extending downward from the lower end of the second extension section, and a second negative electrode column wrapped around the outer periphery of the second connecting column, and the second sealing rubber ring is arranged around the outer periphery of the second extension section.

10. The process for preparing a micro supercapacitor according to claim 8, characterized in that: The second extension section, the second connecting column and the second shell are integrally formed.

Citation Information

Patent Citations

  • Full-sealing nickel-carbon supercapacitor manufacturing method

    CN104752072A

  • Installation-facilitating supercapacitor

    CN105551826A

  • Electrochemical cell and manufacturing method of the same

    JP2021005457A

  • Cable supporting unit for mobile communication equipment with good electrification

    KR102104587B1

  • Capacitor, manufacturing method therefor, and use thereof

    US20230335348A1

Cited By

  • Preparation process of electric energy storage fabric

    CN119008262A

  • A process for the preparation of an electrical energy storage fabric

    CN119008262B