Preparation method of ceramic diaphragm and multilayer chip ceramic capacitor

By using the combination of a protective film and tension suction roller in the preparation of ceramic slurry, the distribution of ceramic slurry is solved, and the corrosion resistance and density of ceramic slurry is improved. , improves the yield rate of multi-layer chip ceramic capacitors.

CN119028743APending Publication Date: 2024-11-26XINWEI ELECTRONIC TECH (YIYANG) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411222130.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the manufacturing process of multi-layer sheet ceramic capacitors, ceramic diaphragms are susceptible to uneven heat, resulting in uneven distribution of organic matter, poor corrosion performance, and affecting yield.

Method used

By using a protective film during the preparation of the ceramic slurry, and using the combination of the casting guide roller and the tension suction roller, the distribution of the ceramic slurry is adjusted, so that the organic matter in the ceramic slurry gathers more away from the protective film The surface improves corrosion resistance and directly dry ceramic slurry through the drying device to reduce heat loss and improve the density and quality of the ceramic diaphragm.

Benefits of technology

It improves the corrosion resistance and density of the ceramic diaphragm, reduces heat loss during the drying process, improves the quality of the ceramic diaphragm and the yield of multi-layer sheet ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028743A_ABST
    Figure CN119028743A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a ceramic diaphragm and a multilayer chip ceramic capacitor. The casting head coats the second surface with ceramic slurry below the second surface. Organic matters in the ceramic slurry are influenced by gravity, and more organic matters are gathered on the surface, far away from the protective film, of the ceramic diaphragm, so that the surface, far away from the protective film, of the prepared ceramic diaphragm is higher in corrosion resistance. The direction of the protective film is adjusted through the first turning roll shaft, so that the second surface faces upwards, and unsolidified organic matters in the ceramic slurry flow to the surface in contact with the protective film, so that the overall compactness of the prepared ceramic diaphragm is more uniform. The second surface faces downwards and passes through the drying device, the ceramic slurry is directly dried by the drying device, heat loss in the drying process is reduced, and the drying efficiency is improved. The ceramic slurry is directly contacted with heat generated by the drying device without being shielded by the protective film, so that the condition of non-uniform heating of the ceramic slurry is reduced, the quality and performance of the ceramic diaphragm are improved, and the damage of high temperature to the protective film can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of preparation of multilayer chip ceramic capacitors, and in particular to a preparation method of a ceramic diaphragm and a multilayer chip ceramic capacitor. Background Art

[0002] Multilayer ceramic capacitors (MLCC) are also called chip capacitors. Chip capacitors have the characteristics of small size, large capacity, and high stability. In the process of manufacturing MLCC, the ceramic slurry is coated on the PET film through the slurry injection port of the casting equipment. After drying, a ceramic diaphragm with a certain thickness, strength, and uniform density is made. However, during the drying process, the ceramic slurry attached to the PET film is prone to uneven heating, and under the influence of gravity, the side of the ceramic diaphragm close to the PET film has more organic matter, and the side away from the PET film has less organic matter. When printing the conductive paste on the ceramic diaphragm, since the solvent in the conductive paste has a certain dissolving effect on the ceramic diaphragm, the side with less organic matter content is corroded more severely, which will cause the thickness uniformity of the ceramic diaphragm to deteriorate, resulting in a decrease in the yield rate of the manufactured ceramic diaphragm. Summary of the invention

[0003] The present application provides a method for preparing a ceramic diaphragm and a multilayer ceramic capacitor, aiming to improve the problems of poor corrosion resistance and uneven thickness of the ceramic diaphragm.

[0004] In the first aspect, the present application provides a method for preparing a ceramic diaphragm, comprising: mixing ceramic raw materials and grinding them to form a ceramic slurry, wherein the ceramic raw materials include ceramic powder, adhesive, first solvent, dispersant and plasticizer. A protective film is provided, wherein the protective film has a first surface and a second surface arranged oppositely in the thickness direction. A casting introduction roller, a casting outlet roller and a casting head are provided, and the first surface portion is abutted against the casting introduction roller and the casting outlet roller, and the casting head is coated with the ceramic slurry on the second surface below the second surface. A first steering roller is provided, and the direction of the protective film is adjusted by the first steering roller, so that the second surface faces upward. A first tension suction roller, a second tension suction roller and a drying device are provided, and a portion of the first surface is abutted against the first tension suction roller and the second tension suction roller, and the direction of the protective film is adjusted by the first tension suction roller, so that the second surface passes through the drying device downward, and the drying device dries the ceramic slurry between the first tension suction roller and the second tension suction roller to obtain a ceramic diaphragm.

[0005] In some embodiments, the drying device includes a first temperature zone, a second temperature zone, and a third temperature zone arranged in sequence, wherein the temperature of the first temperature zone is T1, the temperature of the second temperature zone is T2, the temperature of the third temperature zone is T3, and T1 <T2<T3。

[0006] In some embodiments, after obtaining the ceramic diaphragm, the preparation method further comprises: providing a winding roller, and winding the ceramic diaphragm on the winding roller, wherein the second surface of the protective film faces the winding roller.

[0007] In some embodiments, the protective film includes any one of a PET film, a PI film, a PC film, and a PE film.

[0008] In some embodiments, the ceramic powder includes at least one of aluminum oxide, silicon dioxide, silicon nitride, zirconium oxide, and titanium oxide.

[0009] In some embodiments, the binder includes at least one of polyvinyl alcohol, polyacrylic acid, carboxymethyl cellulose, polyethylene glycol, epoxy resin, and phenolic resin.

[0010] In some embodiments, the dispersant includes at least one of polyacrylates, polyphosphates, fatty acid salts, and silane coupling agents.

[0011] In some embodiments, the plasticizer includes at least one of glycerol, dibutyl phthalate, dioctyl phthalate, polyethylene glycol, lauric acid, and tricresyl phosphate. The first solvent includes at least one of ethanol, isopropanol, toluene, xylene, and toluene.

[0012] In some embodiments, the T1 comprises 30°C to 55°C, the T2 comprises 55°C to 85°C, and the T3 comprises 85°C to 120°C.

[0013] In a second aspect, the present application provides a multilayer ceramic capacitor, comprising a ceramic diaphragm prepared by the preparation method described in any one of the first aspects.

[0014] Different from the related art, the embodiment of the present application provides a method for preparing a ceramic diaphragm. The first surface portion of the protective film is in contact with the casting inlet roller and the casting outlet roller, and the casting head coats the second surface with ceramic slurry below the second surface. In the process of forming the ceramic diaphragm, the organic matter in the ceramic slurry is affected by gravity and gathers more on the surface of the ceramic diaphragm away from the protective film, so that the surface of the prepared ceramic diaphragm away from the protective film has stronger corrosion resistance. The protective film is adjusted in direction by the first steering roller so that the second surface faces upward, and the unsolidified part of the organic matter in the ceramic slurry flows to the surface in contact with the protective film, so that the overall density of the prepared ceramic diaphragm is more uniform. The first tension suction roller can adjust the direction of the protective film so that the second surface passes through the drying device downward, and the second surface is coated with ceramic slurry. The ceramic slurry is directly dried by the drying device, which increases the drying speed of the ceramic slurry, reduces heat loss during the drying process, and improves the drying efficiency. Without the protection film, the ceramic slurry is directly in contact with the heat generated by the drying device, which reduces the uneven heating of the ceramic slurry, improves the quality and performance of the ceramic diaphragm, and reduces the damage to the protective film caused by high temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] One or more embodiments are exemplarily described by corresponding drawings, which do not constitute limitations on the embodiments. Elements with the same reference numerals in the drawings represent similar elements, and the figures in the drawings do not constitute proportional limitations unless otherwise stated.

[0016] Figure 1 is a flow chart of some ceramic diaphragm preparation methods provided in the embodiments of the present application;

[0017] Figure 2 It is a schematic diagram of the structure of some protective films provided in the embodiments of the present application;

[0018] Figure 3 It is a schematic diagram of the structure of some casting equipment provided in the embodiments of the present application;

[0019] Figure 4 is a schematic diagram of the structure of some ceramic diaphragms provided in the embodiments of the present application;

[0020] Figure 5 It is a schematic diagram of the structure of some ceramic diaphragms provided in the embodiments of the present application cast on the second surface;

[0021] Figure 6 It is a schematic diagram of the structure of some casting equipment provided in the embodiments of the present application.

[0022] Description of reference numerals:

[0023] 100. Casting equipment;

[0024] 10. unwinding unit; 11. unwinding roller; 12. deviation correcting device; 121. first roller; 122. second roller; 123. deviation correcting member;

[0025] 20. Casting unit; 21. Casting introduction roller; 22. Casting outlet roller; 23. Casting head; 24. Gear pump; 25. Stirring barrel;

[0026] 30. Drying section; 31. First tension suction roller; 32. Second tension suction roller; 33. Drying device; 331. First temperature zone; 332. Second temperature zone; 333. Third temperature zone;

[0027] 40. winding section; 41. winding roller; 42. third roller; 43. fourth roller;

[0028] 50. first adjustment part; 51. first steering roller; 52. third tension suction roller; 53. fourth tension suction roller;

[0029] 60. second adjustment part; 61. second steering roller; 62. fifth tension suction roller; 63. sixth tension suction roller;

[0030] 200, protective film; 201, first surface; 202, second surface;

[0031] 300, ceramic diaphragm;

[0032] X, first direction. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0034] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "several" and "multiple" is more than two, unless otherwise clearly and specifically defined.

[0035] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0036] Reference to "embodiment" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. In addition, the technical features involved in the different embodiments of the present application described below may be combined with each other as long as they do not conflict with each other.

[0037] In the first aspect, the present application provides a method for preparing a ceramic diaphragm. Figure 1 , Figure 1 Flowcharts of some ceramic diaphragm preparation methods provided in the embodiments of the present application, the preparation method comprising the following steps:

[0038] Step S1: Mixing and grinding ceramic raw materials to form ceramic slurry, the ceramic raw materials include ceramic powder, adhesive, a first solvent, a dispersant and a plasticizer.

[0039] Ceramic powder is the main component for preparing ceramic diaphragms. Ceramic powder forms the basic skeleton of ceramic diaphragms through the mutual accumulation and combination of particles. The properties of ceramic diaphragms prepared by different ceramic powders will be slightly different. Different ceramic powders can be selected according to different needs. For example, ceramic powder includes at least one of aluminum oxide, silicon dioxide, silicon nitride, zirconium oxide, and titanium oxide.

[0040] The adhesive is a viscous substance that can connect multiple separated substances together through viscosity. The adhesive in the embodiment of the present application helps to bind the ceramic powder particles together and improve the strength and shape stability of the ceramic diaphragm. For example, the adhesive includes at least one of polyvinyl alcohol, polyacrylic acid, carboxymethyl cellulose, polyethylene glycol, epoxy resin, and phenolic resin.

[0041] The first solvent can be used to dissolve the ceramic powder and disperse other components to form a uniform slurry system. For example, the first solvent includes at least one of ethanol, isopropanol, toluene, xylene, and toluene.

[0042] Dispersants are surfactants that have two opposite properties, lipophilicity and hydrophilicity, in the molecule. Dispersants can make ceramic powders evenly dispersed in the first solvent, reduce the agglomeration of ceramic powder particles, and improve the stability and uniformity of ceramic slurry. For example, dispersants include at least one of polyacrylates, polyphosphates, fatty acid salts, and silane coupling agents. Among them, polyacrylates include sodium polyacrylate, potassium polyacrylate, etc. Polyphosphates include sodium tripolyphosphate, potassium tripolyphosphate, etc. Fatty acid salts include sodium laurate, potassium laurate, etc. Silane coupling agents include γ-aminopropyl triethoxysilane, γ-glycidyl ether oxypropyl trimethoxysilane, etc.

[0043] Plasticizer is an additive that increases the softness or toughness of a material. Plasticizer can increase the plasticity and flexibility of the ceramic diaphragm and reduce the cracking of the ceramic diaphragm during the molding process. For example, the plasticizer includes at least one of glycerol, dibutyl phthalate, dioctyl phthalate, polyethylene glycol, lauric acid, and tricresyl phosphate.

[0044] For example, the ceramic powder, the binder, the first solvent, the dispersant and the plasticizer can be mixed in a certain ratio according to different needs, and the ceramic raw materials can be evenly mixed by ball grinding to form a ceramic slurry with a certain fluidity.

[0045] Step S2: Provide a protective film, please refer to Figure 2 The protective film 200 has a first surface 201 and a first surface 202 that are oppositely disposed along the thickness direction. The first direction X is the thickness direction.

[0046] The protective film 200 in the embodiment of the present application can provide physical support for the formation of the ceramic diaphragm 300, so that the ceramic slurry can be attached to the protective film 200, and the deformation and cracking can be reduced during the processing and treatment of the ceramic slurry. In addition, the protective film 200 can drive the ceramic diaphragm 300 to move, which is convenient for the operation and transfer of the ceramic diaphragm 300. For example, the protective film 200 includes any one of a thermoplastic polyester (Polyethylene Terephthalate, PET) film, a polyimide film (Polyimide Film, PI film), a polycarbonate film (Polycarbonate Film, PC film), and a polyethylene film (Protective Film, PE film).

[0047] Step S3: Provide a casting inlet roller 21, a casting outlet roller 22 and a casting head 23, and hold the first surface 201 against the casting inlet roller 21 and the casting outlet roller 22. The casting head 23 coats the ceramic slurry on the first surface 202 below the first surface 202.

[0048] Please refer to Figure 3 The casting introduction roller 21, the casting outlet roller 22 and the casting head 23 are all arranged in the casting part 20, and the casting head 23 is arranged between the casting introduction roller 21 and the casting outlet roller 22. The casting introduction roller 21 can accurately introduce the protective film 200 into the casting area to ensure the correctness of the conveying direction and position of the protective film 200. The casting introduction roller 21 and the casting outlet roller 22 respectively apply a certain tension to the protective film 200, so that the protective film 200 maintains a certain flatness and tightness before entering the casting head 23 for casting.

[0049] The cast output roller 22 has the function of driving the lagging protective film 200 to move forward, helping to maintain the shape and size stability of the cast protective film 200 and reducing the deformation and relaxation of the cast protective film 200.

[0050] The casting head 23 is a device for uniformly extruding a liquid or molten slurry to form a continuous film or coating. The casting head 23 is connected to the stirring barrel 25 through a gear pump 24. The ceramic slurry can be continuously stirred uniformly in the stirring barrel 25. The ceramic slurry can be introduced into the casting head 23 through the gear pump 24 to cast the ceramic slurry onto the first surface 202 of the protective film 200.

[0051] Please refer to Figure 4 and Figure 5 , the first surface 201 of the protective film 200 is partially in contact with the casting introduction roller 21 and the casting outlet roller 22, and the casting head 23 coats the first surface 202 with ceramic slurry below the first surface 202 to form a ceramic diaphragm 300. The ceramic slurry contains an adhesive so that the ceramic slurry can adhere to the first surface, and the formed ceramic diaphragm 300 itself is relatively thin, which can reduce the probability of the ceramic slurry falling. In the process of forming the ceramic diaphragm 300, the organic matter in the ceramic slurry is affected by gravity and gathers more on the surface of the ceramic diaphragm 300 away from the protective film 200, rather than the surface of the ceramic diaphragm 300 in contact with the protective film 200, so that the surface of the prepared ceramic diaphragm 300 away from the protective film 200 has stronger corrosion resistance. When printing the conductive slurry on the ceramic diaphragm 300, the erosion of the solvent in the conductive slurry can be reduced, and the yield rate of the ceramic diaphragm 300 can be improved.

[0052] In some embodiments, please refer to Figure 3 Before the protective film 200 is cast, the preparation method further includes providing a roll-out section 10, which is arranged before the casting section 20. The roll-out section 10 includes a roll-out roller 11, on which the protective film 200 is wound, and the roll-out roller 11 can roll the protective film 200 to the casting section 20. The roll-out roller 11 can provide support for the winding and unwinding of the protective film 200, ensuring that the protective film 200 remains stable during movement and reduces sagging, twisting and the like. The roll-out roller 11 can be connected to a driving device, which provides power to the roll-out roller 11, thereby controlling the winding or unwinding speed and tension of the protective film 200, ensuring the smoothness and precision of the entire process.

[0053] Step S4: Please refer to Figure 3 A first steering roller 51 is provided, and the direction of the protective film 200 is adjusted by the first steering roller 51 so that the first surface 202 faces upward.

[0054] The first steering roller 51 turns the direction of the cast protective film 200 so that the first surface 202 faces upward, and the unsolidified organic flow in the ceramic slurry can flow to the surface in contact with the protective film 200, so that the overall density of the prepared ceramic diaphragm 300 is more uniform. After the protective film 200 is turned, the first surface 202 and the adhesive in the ceramic slurry are more firmly bonded under the action of gravity, which can reduce the situation where the protective film 200 enters the drying device and falls. By adjusting the rotation direction of the protective film 200 through the first steering roller 51, each device is more compact, saving operating space and floor space.

[0055] In some embodiments, please refer to Figure 6 , a third tension suction roller 52 and a fourth tension suction roller 53 are provided, and the third tension suction roller 52, the fourth tension suction roller 53 and the first steering roller shaft 51 are all arranged on the first adjustment part 50. The protective film 200 is arranged on the first steering roller shaft 51, the third tension suction roller 52 and the fourth tension suction roller 53 in sequence. Part of the first surface 201 is against the first steering roller shaft 51, the third tension suction roller 52 and the fourth tension suction roller 53. When the protective film 200 moves between the third tension suction roller 52 and the fourth tension suction roller 53, the third tension suction roller 52 and the fourth tension suction roller 53 are located on the same horizontal line, so that the first surface 202 is in a horizontal state when facing upward. When the ceramic slurry passes through the first steering roller shaft 51, the third tension suction roller 52 and the fourth tension suction roller 53, a small part of the unsolidified organic matter in the ceramic slurry will precipitate on the surface in contact with the protective film 200, thereby enhancing the overall corrosion resistance of the ceramic diaphragm 300 and making the density of the ceramic diaphragm 300 more uniform.

[0056] The third tension suction roller 52 can also provide tension to the protective film 200, so that the protective film 200 maintains a certain degree of tension during the movement, reducing the problems of looseness and wrinkles of the protective film 200. In addition, the third tension suction roller 52 can pull the protective film 200 out from the previous process, playing a certain role in excessive traction. The fourth tension suction roller 53 can cooperate with the third tension suction roller 52 to adjust the tension level of the protective film 200 and adaptively correct the problems of the protective film 200 that may deviate from the running track.

[0057] Step S5: Please refer to Figure 3 A first tension suction roller 31, a second tension suction roller 32 and a drying device 33 are provided, and a portion of the first surface 201 is held against the first tension suction roller 31 and the second tension suction roller 32. The direction of the protective film 200 is adjusted by the first tension suction roller 31 so that the first surface 202 passes through the drying device 33 downward. The drying device 33 dries the ceramic slurry between the first tension suction roller 31 and the second tension suction roller 32 to obtain a ceramic diaphragm 300.

[0058] The first tension suction roller 31, the second tension suction roller 32 and the drying device 33 are all arranged in the drying section 30. The first tension suction roller 31 can adjust the direction of the protective film 200 so that the first surface 202 faces downward and faces the drying device 33. The first tension suction roller 31 can also provide tension to the protective film 200 so that the protective film 200 maintains a certain degree of tension during movement, reducing problems such as slack and wrinkles of the protective film 200. The first tension suction roller 31 can pull out the protective film 200 from the previous process, playing a certain role in traction and transition. The second tension suction roller 32 can cooperate with the first tension suction roller 31 to adjust the tension level of the protective film 200 and adaptively correct the problem that the protective film 200 may deviate from the running track.

[0059] The drying device 33 can evaporate a large amount of moisture in the ceramic slurry and remove the solvent, so that the ceramic slurry forms a ceramic film 300 on the first surface 202. The first surface 202 faces the drying device 33, and the first surface 202 is coated with the ceramic slurry. The ceramic slurry is directly dried by the drying device 33, which improves the drying speed of the ceramic slurry, reduces heat loss during drying, and improves drying efficiency. Without the protection of the protective film 200, the ceramic slurry directly contacts the heat generated by the drying device 33, reducing the uneven heating of the ceramic slurry, improving the quality and performance of the ceramic film 300, and also reducing the damage to the protective film 200 caused by high temperature.

[0060] In some embodiments, please refer to Figure 3 , the drying device 33 includes a first temperature zone 331, a second temperature zone 332 and a third temperature zone 333 arranged in sequence. The temperature of the first temperature zone 331 is T1, the temperature of the second temperature zone 332 is T2, and the temperature of the third temperature zone 333 is T3, where T1 < T2 < T3. The protective film 200 is arranged in the first temperature zone 331, the second temperature zone 332 and the third temperature zone 333 in sequence. For example, the first temperature zone 331 is a low-temperature zone with a temperature set at 30°C to 55°C. The second temperature zone 332 is a medium-temperature zone with a temperature set at 55°C to 85°C. The third temperature zone 333 is a high-temperature zone with a temperature set at 85°C to 120°C.

[0061] The embodiment of the present application provides a method for preparing a ceramic diaphragm 300. The first surface 201 of the protective film 200 is partially in contact with the casting introduction roller 21 and the casting outlet roller 22, and the casting head 23 coats the first surface 202 with ceramic slurry below the first surface 202. During the process of forming the ceramic diaphragm 300, the organic matter in the ceramic slurry is affected by gravity and more is gathered on the surface of the ceramic diaphragm 300 away from the protective film 200, so that the surface of the prepared ceramic diaphragm 300 away from the protective film 200 has stronger corrosion resistance. The protective film 200 is adjusted in direction by the first steering roller 51 so that the first surface 202 faces upward, and the unsolidified part of the organic matter in the ceramic slurry flows to the surface in contact with the protective film 200, so that the overall density of the prepared ceramic diaphragm 300 is more uniform. The first tension suction roller 31 can adjust the direction of the protective film 200 so that the first surface 202 passes through the drying device 33 downward. The first surface 202 is coated with ceramic slurry, and the ceramic slurry is directly dried by the drying device 33, thereby increasing the drying speed of the ceramic slurry, reducing heat loss during the drying process, and improving the drying efficiency. Without the shielding of the protective film 200, the ceramic slurry directly contacts the heat generated by the drying device 33, reducing the uneven heating of the ceramic slurry, improving the quality and performance of the ceramic diaphragm 300, and reducing the damage of the protective film 200 to high temperature.

[0062] In some embodiments, please refer to Figure 3 After obtaining the ceramic diaphragm 300, the preparation method further includes providing a winding roller 41 and winding the ceramic diaphragm 300 on the winding roller 41. The winding roller 41 is arranged on the winding portion 40, and the first surface 202 of the protective film 200 faces the winding roller 41. The wound ceramic diaphragm 300 is convenient for storage, transportation and subsequent processing. The winding roller 41 can be connected to a driving device, and the driving device provides power to the winding roller 41, so as to control the winding speed and tension of the ceramic diaphragm 300 on the protective film 200, thereby ensuring the smoothness and precision of the whole process.

[0063] In some embodiments, please refer to Figure 6 The unwinding section 10 also provides a deviation correction device 12. The deviation correction device 12 is a device for automatically correcting the deviation of the protective film 200 from a predetermined path during the transmission process. The deviation correction device 12 is arranged between the unwinding roller 11 and the casting introduction roller 21 to reduce the deviation problem of the protective film 200 during casting.

[0064] For further information, please refer to Figure 6The deviation-correcting device 12 also provides a first roller 121, a second roller 122 and a deviation-correcting member 123. The deviation-correcting member 123 is arranged between the first roller 121 and the second roller 122. The protective film 200 passes through the first roller 121, the second roller 122 and the deviation-correcting member 123 in sequence. The first roller 121 and the second roller 122 can adjust the movement direction of the protective film 200. Among them, part of the first surface 201 is against the first roller 121, and the first roller 121 can produce a certain degree of extrusion on the first surface 201, which is helpful to shape and stabilize the shape and thickness of the protective film 200. In the process of extrusion with the first surface 201, part of the bubbles can be discharged from the first surface 201, eliminating the small defects and unevenness of the first surface 201. Part of the first surface 202 is against the second roller 122. Similar to the function of the first roller 121, the second roller 122 can exert a certain amount of extrusion on the first surface 202, which helps to shape and stabilize the shape and thickness of the protective film 200. During the extrusion process with the first surface 202, some bubbles can be discharged from the first surface 202, thereby eliminating minor flaws and unevenness of the first surface 202.

[0065] In some embodiments, please refer to Figure 3 The preparation method further includes providing a second steering roller 61, which is disposed between the winding roller 41 and the second tension suction roller 32. The direction of the protective film 200 is adjusted by the second steering roller 61 so that the first surface 202 of the protective film 200 faces the winding roller 41, so that the ceramic diaphragm 300 attached to the wound protective film 200 faces inward, thereby reducing the damage and moisture of the ceramic diaphragm 300 during storage and transportation. The protective film 200 is sequentially disposed on the second tension suction roller 32, the second steering roller 61 and the winding roller 41. The first surface 201 abuts against the second tension suction roller 32 and the winding roller 41, and the first surface 202 abuts against the second steering roller 61.

[0066] In some embodiments, please refer to Figure 6 The preparation method further includes providing a fifth suction roller 62 and a sixth tension suction roller 63. The second steering roller shaft 61, the fifth suction roller 62 and the sixth tension suction roller 63 are all arranged on the second adjustment part 60. The protective film 200 is arranged on the second steering roller shaft 61, the fifth suction roller 62 and the sixth tension suction roller 63 in sequence. The first surface 202 abuts against the second steering roller shaft 61, the fifth suction roller 62 and the sixth tension suction roller 63. Among them, the fifth suction roller 62 has a similar function to the first tension suction roller 31, and the sixth tension suction roller 63 has a similar function to the second tension suction roller 32.

[0067] In some embodiments, please refer to Figure 6The winding section 40 also provides a third roller 42 and a fourth roller 43, which are both arranged between the winding roller 41 and the sixth tension suction roller 63, and the protective film 200 is arranged on the sixth tension suction roller 63, the third roller 42 and the fourth roller 43 in sequence. The third roller 42 and the fourth roller 43 can adjust the movement direction of the protective film 200. Among them, the first surface 201 is against the third roller 42, and the first surface 202 is against the fourth roller 43 and the sixth tension suction roller 63. After the adjustment of the third roller 42 and the fourth roller 43, the ceramic diaphragm 300 attached to the wound protective film 200 faces inward, reducing the damage and moisture of the ceramic diaphragm 300 during storage and transportation. In addition, the dried ceramic diaphragm 300 is squeezed by the fourth roller 43, which can discharge some bubbles from the first surface 202, eliminating the tiny flaws and unevenness on the surface of the ceramic diaphragm 300. The third roller 42 and the fourth roller 43 support the protective film 200 , thereby ensuring the smooth transportation of the ceramic diaphragm 300 .

[0068] In a second aspect, an embodiment of the present application provides a multilayer ceramic capacitor, comprising a ceramic diaphragm 300 prepared by any preparation method according to the first aspect.

[0069] In a third aspect, an embodiment of the present application provides a casting device 100, which is used to prepare a ceramic diaphragm 300 using any preparation method of the first aspect.

[0070] The preparation method of the ceramic diaphragm is described below in conjunction with a specific embodiment:

[0071] Example 1

[0072] (1) 1000 g of barium titanate powder, 1000 g of toluene, 1000 g of ethanol, 20 g of dibutyl phthalate, 150 g of polyvinyl butyral, and 10 g of sodium polyacrylate were weighed, mixed, and ground with a grinding ball to form a ceramic slurry.

[0073] (2) A PET film is provided, the PET film having a first surface and a second surface in a thickness direction.

[0074] (3) A casting inlet roller, a casting outlet roller and a casting head are provided, the first surface portion is abutted against the casting inlet roller and the casting outlet roller, and the casting head is located below the second surface to coat the ceramic slurry on the second surface.

[0075] (4) A first steering roller is provided, and the direction of the PET film is adjusted by the first steering roller so that the second surface of the PET film faces upward.

[0076] (5) Provide a first tension suction roller, a second tension suction roller and a drying device, hold a portion of the first surface of the PET film against the first tension suction roller and the second tension suction roller, and adjust the direction of the PET film through the first tension suction roller so that the second surface passes through the drying device downward. The drying device dries the ceramic slurry between the first tension suction roller and the second tension suction roller to obtain a ceramic film sheet.

[0077] (6) Nickel electrode slurry is screen-printed on the ceramic diaphragm, and after drying, the nickel electrode slurry forms an inner electrode layer on the ceramic diaphragm.

[0078] (7) A plurality of ceramic diaphragms with inner electrode layers are stacked, pressed, debonded and sintered to obtain a ceramic chip, and the ends of the ceramic chip are coated and sintered with external electrodes to form a multi-layer ceramic capacitor.

[0079] Comparative Example 1

[0080] (1) 1000 g of barium titanate powder, 1000 g of toluene, 1000 g of ethanol, 20 g of dibutyl phthalate, 150 g of polyvinyl butyral, and 10 g of sodium polyacrylate were weighed, mixed, and ground with a grinding ball to form a ceramic slurry.

[0081] (2) A PET film is provided, the PET film having a first surface and a second surface in a thickness direction.

[0082] (3) A casting introduction roller, a casting outlet roller and a casting head are provided, the first surface portion is abutted against the casting introduction roller and the casting outlet roller, and the casting head is disposed above the first surface to coat the ceramic slurry on the first surface.

[0083] (4) Provide a first tension suction roller, a second tension suction roller and a drying device, and hold a portion of the first surface of the PET film against the first tension suction roller and the second tension suction roller. The drying device is located below the second surface and faces away from the ceramic slurry. The drying device dries the ceramic slurry between the first tension suction roller and the second tension suction roller to obtain a ceramic membrane sheet.

[0084] (6) Nickel electrode slurry is screen-printed on the ceramic diaphragm, and after drying, the nickel electrode slurry forms an inner electrode layer on the ceramic diaphragm.

[0085] (7) A plurality of ceramic diaphragms with inner electrode layers are stacked, pressed, cut, debonded and sintered to obtain a ceramic chip, and the ends of the ceramic chip are coated and sintered with external electrodes to form a multilayer ceramic capacitor.

[0086] The following tests were performed on the multilayer ceramic capacitors prepared in Example 1 and Comparative Example 1 respectively:

[0087] (1) Breakdown voltage test: 10 multilayer ceramic capacitors prepared in Example 1 and Comparative Example 1 were selected respectively, and the breakdown voltage of the products was tested using a ZJC-100KV voltage tester. The test samples were clamped with an instrument lead clamp and the voltage rate was 5V / s until the capacitor was broken down. The breakdown voltage value was recorded, wherein the instrument current was set to DC.

[0088] (2) Reliability test: 100 pieces of multilayer ceramic capacitors prepared in Example 1 and Comparative Example 1 were selected respectively, and the reliability of the multilayer ceramic capacitors was tested using a ZJC-100KV voltage tester and an oven. The multilayer ceramic capacitors were welded on a PCB board, the positive and negative electrodes of the withstand voltage tester were welded to the positive and negative electrodes of the PCB, the PCB was immersed in silicone oil, and placed in an oven, wherein the oven temperature was 120°C and the voltage was twice the rated voltage.

[0089] The breakdown voltages of the 10 multilayer ceramic capacitors in Example 1 are 118V, 120V, 123V, 124V, 122V, 118V, 124V, 125V, 117V and 119V, respectively. The average breakdown voltage of the multilayer ceramic capacitors in the above Example 1 is 121V, and the range is 8V. The breakdown voltages of the 10 multilayer ceramic capacitors in Comparative Example 1 are 101V, 98V, 108V, 120V, 107V, 112V, 114V, 99V, 110V, 112V and 111V, respectively. The average breakdown voltage of the multilayer ceramic capacitors in Comparative Example 1 is 108V, and the range is 22V. There are no failed particles in the 100 multilayer ceramic capacitors in Example 1. Three failed particles were found in the 100 multilayer ceramic capacitors in Comparative Example 1.

[0090] According to the breakdown voltage and reliability test results, the breakdown voltage of the multilayer ceramic capacitor of Example 1 is higher than that of the multilayer ceramic capacitor in Comparative Example 1, and the breakdown voltage in Example 1 is more concentrated, and there are no failed particles, indicating that the multilayer ceramic capacitor in Example 1 has better performance, the yield rate of the multilayer ceramic capacitor in Example 1 is higher, and the thickness of the ceramic diaphragm is more uniform. The breakdown voltage of the multilayer ceramic capacitor in Comparative Example 1 is lower, and the breakdown voltage is more dispersed, and there are invalid particles. The possible reason is that the ceramic slurry in Comparative Example 1 is cast above the first surface, so that more organic matter in the ceramic diaphragm is precipitated to the surface in contact with the PET film, and the surface of the ceramic diaphragm away from the PET film has less chance content, and the ceramic slurry in Comparative Example 1 is dried with its back to the drying device, the ceramic diaphragm is heated unevenly, the organic matter is not dried thoroughly, and the anti-etching ability is poor, so that the thickness uniformity of the ceramic diaphragm is poor, and the yield rate of the prepared multilayer ceramic capacitor is low.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Under the concept of the present application, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present application as described above, which are not provided in detail for the sake of simplicity. Although the present application has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for preparing a ceramic diaphragm, characterized in that: include: Mixing and grinding ceramic raw materials to form ceramic slurry, wherein the ceramic raw materials include ceramic powder, a binder, a first solvent, a dispersant and a plasticizer; Providing a protective film, wherein the protective film has a first surface and a second surface disposed opposite to each other in a thickness direction; Providing a casting introduction roller, a casting outlet roller and a casting head, the first surface portion is held against the casting introduction roller and the casting outlet roller, and the casting head is below the second surface to coat the ceramic slurry on the second surface; Providing a first steering roller, through which the direction of the protective film is adjusted so that the second surface faces upward; A first tension suction roller, a second tension suction roller and a drying device are provided, and part of the first surface is pressed against the first tension suction roller and the second tension suction roller. The direction of the protective film is adjusted by the first tension suction roller so that the second surface passes through the drying device downward. The drying device dries the ceramic slurry between the first tension suction roller and the second tension suction roller to obtain a ceramic diaphragm.

2. The preparation method according to claim 1, characterized in that: The drying device comprises a first temperature zone, a second temperature zone and a third temperature zone arranged in sequence, wherein the temperature of the first temperature zone is T1, the temperature of the second temperature zone is T2, the temperature of the third temperature zone is T3, and T1 <T2<T3。 3. The preparation method according to claim 1, characterized in that: After obtaining the ceramic diaphragm, the preparation method further comprises: Providing a winding roller shaft, and winding the ceramic diaphragm around the winding roller shaft; Wherein, the second surface of the protective film faces the winding roller axis.

4. The preparation method according to claim 1, characterized in that: The protective film includes any one of a PET film, a PI film, a PC film, and a PE film.

5. The preparation method according to claim 1, characterized in that: The ceramic powder includes at least one of barium titanate, aluminum oxide, silicon dioxide, silicon nitride, zirconium oxide, and titanium oxide.

6. The preparation method according to claim 1, characterized in that: The adhesive comprises at least one of polyvinyl alcohol, polyacrylic acid, carboxymethyl cellulose, polyethylene glycol, epoxy resin and phenolic resin.

7. The preparation method according to claim 1, characterized in that: The dispersant includes at least one of polyacrylates, polyphosphates, fatty acid salts and silane coupling agents.

8. The preparation method according to claim 1, characterized in that: The plasticizer includes at least one of glycerol, dibutyl phthalate, dioctyl phthalate, polyethylene glycol, lauric acid, and tricresyl phosphate; The first solvent includes at least one of ethanol, isopropanol, toluene, xylene, and toluene.

9. The preparation method according to claim 2, characterized in that: The T1 includes 30°C to 55°C, the T2 includes 55°C to 85°C, and the T3 includes 85°C to 120°C.

10. A multilayer ceramic capacitor, characterized in that: A ceramic diaphragm prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Water-based adhesive for chip multilayer ceramic capacitor and preparation method of water-based adhesive

    CN119875540A