Solar cell and preparation method thereof
By simplifying the preparation process of solar cells, using polishing and printing technology to form doped regions and performing high-temperature annealing, the problems of complex and high cost of existing processes are solved, efficient and low-cost solar cell production is achieved, and product quality is improved. rate and efficiency.
Patent Information
- Application Number
- CN202411210439.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The preparation process of existing solar cells is complex and has high costs, which leads to increased equipment investment and production costs, serious problems in automation pollution and debris, and low yields.
The silicon substrate is polished and treated, and the tunneled oxide layer and intrinsic polysilicon layer are deposited. The patterned doped regions are formed by spraying or screen printing of boron and phosphorus paste, and the boron and phosphorus diffusion is carried out in combination with high-temperature annealing to simplify the process flow. And the metal grid lines are printed on the PN junction for sintering.
The preparation process of solar cells has been greatly simplified, production costs have been reduced, product performance has been improved, suitable for large-scale production, and yield and efficiency have been improved.
Smart Images

Figure CN119029065A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photovoltaic solar cells, and in particular to a solar cell and a method for preparing the same. Background Art
[0002] Solar cells are devices that can convert light energy into electrical energy. When the cell is exposed to light, the cell substrate absorbs photons to generate electron-hole pairs. The hole pairs are separated under the action of the built-in electric field of the PN junction and are led out through the emitter and back field of the solar cell. They are finally collected and transmitted to the outside by the electrodes set on the substrate. Solar cells have developed from the earliest aluminum back field cells to PERC cells and then to the current mainstream TOPCON / HIT cells. The cell efficiency has increased from about 16% to the current nearly 26% cell efficiency. As a platform technology, the BC (Back Contact) cell structure can be combined with the TOPCON and HIT structures (combined with TOPCON is called TBC, combined with HIT is called HBC, so some companies also call it XBC). This type of cell puts the core structure of the cell PN junction, that is, the cell emitter and base, on the back, and there is no shielding on the front of the cell, which increases the short-circuit current. Therefore, BC cells have the advantages of beautiful appearance, high cell efficiency and stronger power generation capacity, and are generally considered to be the most important next-generation cell technology.
[0003] Conventional processes require the preparation of boron-doped polysilicon, also known as P-type silicon, on the entire surface, and then grooves are made in the area where N-type silicon is to be prepared. The general method is to prepare the area where N-type silicon is to be prepared by laser etching or by preparing a mask first and then chemically etching. The current disadvantages of laser etching are: low production capacity, damage that reduces battery efficiency; the mask + chemical etching process is complex and costly. This process is extremely complex and costly, and the process itself leads to more pollution and debris in the process itself and the automation used, and it is difficult to increase the yield caused by the process itself.
[0004] Therefore, there is an urgent need for a solar cell and a preparation method thereof that can reduce equipment investment, production cost, plant investment, and improve yield. Summary of the invention
[0005] In view of the shortcomings of the prior art described above, the purpose of the present application is to provide a solar cell and a method for preparing the same, so as to solve the problems that the process flow of existing solar cells is extremely complex and costly during production, the process flow often leads to more pollution and debris in the process itself and the automation used, and the yield is low due to the process itself.
[0006] To achieve the above-mentioned object and other related objects, the present application provides a method for preparing a solar cell, characterized in that it comprises the following steps: Providing a silicon substrate, and polishing the front and back sides of the silicon substrate; Depositing a tunnel oxide layer and an intrinsic polysilicon layer in sequence along the thickness direction on the back side of the silicon substrate; Boron slurry is spray-printed or screen-printed according to a pattern on the back side of the intrinsic polysilicon layer away from the silicon substrate, and a patterned boron layer is formed after drying, wherein the dried boron layer has a gap region to be doped with n-type; In the gap area of the boron layer, phosphorus paste is spray-printed or screen-printed according to a pattern, and dried to form a patterned phosphorus layer; The back side of the intrinsic polysilicon layer is subjected to boron diffusion doping treatment and phosphorus diffusion doping treatment to form a PN junction on the back side of the intrinsic polysilicon layer; the PN junction includes a first conductive doping structure and a second conductive doping structure arranged in a staggered manner in a finger-like cross-shaped manner, and the back side of the first conductive doping structure away from the silicon substrate forms borosilicate glass, and the back side of the second conductive doping structure away from the silicon substrate forms phosphorus silicon glass; Isolating the first conductive doping structure and the second conductive doping structure to expose the silicon substrate corresponding to the boundary region between the first conductive doping structure and the second conductive doping structure; removing the borosilicate glass on the first conductive doping structure, and removing the phosphosilicate glass on the second conductive doping structure; Coating the front and back sides of a silicon substrate; The metal grid line is printed on the PN junction and sintered to prepare the solar cell.
[0007] As a preferred embodiment of the present invention, the silicon substrate is an N-type silicon wafer.
[0008] As a preferred embodiment of the present invention, the front and back sides of the silicon substrate are cleaned before being polished. The silicon substrate can be cleaned using ozone, hydrogen chloride and water.
[0009] As a preferred embodiment of the present invention, the step of polishing the front and back sides of the silicon substrate is performed according to the following method: At a temperature of 55-70°C, a polishing additive with a volume concentration of 0.2%-1% is added to a 2%-8% NaOH aqueous solution or a 4-10% KOH aqueous solution to polish a silicon substrate for 200-300 seconds to prepare a polished surface with a reflectivity of 35-45%.
[0010] As a preferred embodiment of the present invention, the NaOH aqueous solution is prepared by using NaOH as a stock solution with a mass concentration of 40% to 48%; the KOH aqueous solution is prepared by using KOH as a KOH stock solution with a mass concentration of 45% to 50%.
[0011] As a preferred embodiment of the present invention, the step of polishing the front and back sides of the silicon substrate is performed as follows: at a temperature of 60° C., a polishing additive having a volume concentration of 0.4% is added to a NaOH aqueous solution having a volume concentration of 5% to polish the silicon substrate for 200 to 300 seconds to prepare a polished surface having a reflectivity of 35 to 45%.
[0012] As a preferred embodiment of the present invention, a tunnel oxide layer and an intrinsic polysilicon layer are sequentially deposited along the thickness direction on the back side of the silicon substrate by one of LPCVD, PECVD and PVD methods, wherein the tunnel oxide layer is composed of SiO2 and has a thickness of 0.8-1.6 nm; When the tunnel oxide layer is deposited by LPCVD, the deposition temperature is 550-750° C., and the deposition time is 10-40 min. When the intrinsic polysilicon layer is deposited by LPCVD, the thickness of the intrinsic polysilicon layer is 50-150 nm, the deposition temperature is 580-680° C., and the deposition time is 30-90 min. When the tunnel oxide layer is deposited by PECVD, the deposition temperature is 350-500°C and the deposition time is 5-30 minutes; when the intrinsic polysilicon layer is deposited by PECVD, the thickness of the intrinsic polysilicon layer is 50-150 nm, the deposition temperature is 350-500°C and the deposition time is 20-70 minutes; When the tunnel oxide layer is deposited by PVD, the deposition temperature is PVD150~300°C and the deposition time is 3~25min; when the intrinsic polysilicon layer is deposited by PVD, the thickness of the intrinsic polysilicon layer is 50~150nm, the deposition temperature is 150~350°C and the deposition time is 5~30min.
[0013] As the preferred embodiment of the present invention, the boron slurry is composed of a mixture of an organic solvent (such as propylene glycol phenyl ether and / or diethylene glycol butyl ether acetate) and boron powder, and has a certain rheological property for printing or spraying and other processes, and the mass ratio of boron element in the boron slurry is not less than 10%, the drying temperature is 50~200℃, and the drying time is 1~10min; the phosphorus slurry is composed of a mixture of an organic solvent (such as propylene glycol phenyl ether and / or diethylene glycol butyl ether acetate) and phosphorus powder, and has a certain rheological property for printing or spraying and other processes, and the mass ratio of phosphorus element in the phosphorus slurry is not less than 10%, the drying temperature is 50~200℃, and the drying time is 1~10min. By improving the boron slurry and the boron slurry as mentioned above, when the method prepares solar cells, the intrinsic polycrystalline silicon layer on the silicon substrate can be simultaneously diffused with boron and phosphorus under the same thermal diffusion conditions, which greatly simplifies the process flow and provides the possibility for subsequent large-scale production.
[0014] As a preferred embodiment of the present invention, in the steps of performing boron diffusion doping treatment and phosphorus diffusion doping treatment on the back side of the intrinsic polysilicon layer, the annealing temperature required for diffusion is controlled at 850-1100° C. and the annealing time is 30-90 minutes.
[0015] As a preferred embodiment of the present invention, in the steps of performing boron diffusion doping treatment and phosphorus diffusion doping treatment on the back side of the intrinsic polysilicon layer, the annealing temperature required for diffusion is controlled at 850-1050°C.
[0016] As a preferred embodiment of the present invention, the first conductive doping structure and the second conductive doping structure are isolated to prevent contact leakage between the first conductive doping structure and the second conductive doping structure, thereby affecting battery performance. The specific operation steps are as follows: Laser etching is used to perform etching along the boundary between the first conductive doping structure and the second conductive doping structure until the silicon substrate corresponding to the boundary area between the first conductive doping structure and the second conductive doping structure is exposed, a groove is formed at the boundary between the first conductive doping structure and the second conductive doping structure, and passivation of the groove area is completed in a subsequent process, so that an isolation area is formed at the boundary between the first conductive doping structure and the second conductive doping structure.
[0017] As a preferred embodiment of the present invention, before the phosphorus paste is sprayed or screen-printed in the gap area of the boron layer according to a pattern, a mask layer is formed at the boundary of the gap area by screen printing, inkjet printing, or glue coating, exposure and development.
[0018] As a preferred embodiment of the present invention, the isolation treatment step of the first conductive doping structure and the second conductive doping structure is performed according to the following method: The mask layer between the junctions of the first conductive doping structure and the second conductive doping structure is removed, so that an isolation region is formed on the junctions of the first conductive doping structure and the second conductive doping structure.
[0019] As a preferred embodiment of the present invention, the steps of removing the borosilicate glass on the first conductive doping structure and removing the phosphosilicate glass on the second conductive doping structure are performed according to the following method: The silicon substrate after isolation treatment is etched with HF solution with a mass concentration of 15-40%, and the borosilicate glass and phosphosilicate glass formed on the surface of the silicon substrate after high-temperature annealing, as well as the impurities generated by laser etching isolation, are cleaned off.
[0020] As a preferred embodiment of the present invention, the steps of coating the front and back sides of the silicon substrate include: A silicon nitride film is deposited on the front side of the silicon substrate by PECVD, the thickness of the silicon nitride film is controlled to be 70-90 nm, and the refractive index is controlled to be between 1.95 and 2.2; A silicon nitride film and an aluminum oxide film are sequentially deposited on the back side of a silicon substrate along a thickness direction by using a PECVD method, wherein the thickness of the silicon nitride film is controlled to be between 70 and 90 nm, and the refractive index is controlled to be between 1.95 and 2.2; the deposition thickness of the aluminum oxide film is controlled to be between 5 and 35 nm.
[0021] As a preferred embodiment of the present invention, the steps of printing a metal grid line on the PN junction and performing sintering include: Silver paste grid lines are printed on the PN junction by screen printing, the width of the silver paste grid lines is 20~80μm, and the silver paste grid lines are sintered at 700~850℃.
[0022] As a preferred embodiment of the present invention, the front side of the silicon substrate needs to be textured before coating the front side and back side of the silicon substrate, so as to form a pyramid texture surface on the front side of the silicon substrate to increase light absorption.
[0023] Specific texturing method: At a temperature of 75~85°C, use a 3%~20% by volume NaOH aqueous solution (wherein NaOH is a stock solution with a mass concentration of 40%~48%) or a 4~25% KOH aqueous solution (wherein KOH is a KOH stock solution with a mass concentration of 45%~50%), add a 0.2%~2% by volume texturing additive (such as texturing additives from brands such as Shichuang / Tobang / Sanfeng), and texturing the front side of the silicon for 300~500s to prepare a velvet surface with a reflectivity of 9~12%.
[0024] A second object of the present invention is to provide a solar cell, characterized in that it includes a solar cell prepared by the solar cell preparation method described in the present application.
[0025] The solar cell of the present invention is characterized by comprising: Silicon substrate; A tunneling oxide layer formed on the back side of the silicon substrate; An intrinsic polysilicon layer formed on the back side of the tunnel oxide layer away from the silicon substrate; A PN junction is formed on the back side of the intrinsic polysilicon layer away from the silicon substrate; the PN junction comprises a first conductive doping structure and a second conductive doping structure which are arranged in a staggered manner in a finger-like cross-shaped manner, and an isolation region is provided between the first conductive doping structure and the second conductive doping structure; A first passivation anti-reflection layer formed on the front side of the silicon substrate; A second passivation anti-reflection layer formed on the back side of the silicon substrate; and / or A metal gate line formed on a PN junction.
[0026] As a preferred embodiment of the present invention, the silicon substrate is an N-type silicon wafer.
[0027] As a preferred embodiment of the present invention, the thickness of the tunnel oxide layer is 0.8-1.6 nm.
[0028] As a preferred embodiment of the present invention, the thickness of the tunneling oxide layer is 1.2 nm.
[0029] As a preferred embodiment of the present invention, the thickness of the intrinsic polysilicon layer is 50-150 nm.
[0030] As a preferred embodiment of the present invention, the thickness of the intrinsic polysilicon layer is 120 nm.
[0031] As a preferred embodiment of the present invention, the first passivation anti-reflection layer is a silicon nitride film deposited on the front side of the silicon substrate by PECVD, the thickness of the silicon nitride film is controlled to be 70-90 nm, and the refractive index is controlled to be between 1.95 and 2.2.
[0032] As a preferred embodiment of the present invention, a pyramid velvet surface is formed between the front side of the silicon substrate and the first passivation anti-reflection layer, and the reflectivity of the pyramid velvet surface is 9-12%.
[0033] As a preferred embodiment of the present invention, the second passivation anti-reflection layer comprises a silicon nitride film and an aluminum oxide film sequentially deposited along the thickness direction of the silicon substrate, wherein the thickness of the silicon nitride film is controlled to be between 70 and 90 nm, and the refractive index is controlled to be between 1.95 and 2.2; the deposition thickness of the aluminum oxide film is controlled to be between 5 and 35 nm.
[0034] The beneficial effects of the present application are as follows: the present application performs boron doping and phosphorus doping in one step by locally coating phosphorus slurry and boron slurry in a directional manner and combining high-temperature annealing to simultaneously diffuse phosphorus and boron. There is no need to perform boron doping and phosphorus doping in separate steps, which greatly simplifies the preparation process of BC batteries, reduces production costs, and saves equipment costs. The solar cells prepared by this method have good performance and are suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Shown is a schematic diagram of the manufacturing process of a solar cell according to an embodiment of the present application.
[0036] Figure 2 Shown is a structural diagram of a solar cell according to an embodiment of the present application.
[0037] In the accompanying drawings, 1-silicon substrate; 2-tunneling oxide layer; 3-intrinsic polysilicon layer; 4-PN junction; 41-first conductive doping structure; 42-second conductive doping structure; 5-first passivation anti-reflection layer; 6-second passivation anti-reflection layer; 61-silicon nitride film; 62-aluminum oxide film; 7-metal gate line. DETAILED DESCRIPTION
[0038] The following describes the implementation of the present application through specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. The present application can also be implemented or applied through other different specific implementations, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application.
[0039] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0040] In addition, it should be understood that one or more method steps mentioned in this application do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in this application does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these two explicitly mentioned devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of implementation of this application. Changes or adjustments in their relative relationships shall also be regarded as the scope of implementation of this application without substantial changes in the technical content.
[0041] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0042] In the description of the present application, it should be understood that the terms "upper", "lower", "left", "right", "inner", "outer", "axial", "circumferential", etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present application, unless otherwise specified, "multiple" means two or more.
[0043] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0044] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0045] The present application is further described below in conjunction with specific embodiments, but the protection scope of the present application is not limited thereto.
[0046] See also Figure 1 , Figure 1 It is a flow chart of a manufacturing method of a solar cell of the present application. It should be noted that if there is substantially the same result, the method of the present application is not limited to Figure 1 The process sequence shown is limited.
[0047] See also Figure 1 This embodiment provides a method for manufacturing a solar cell, comprising the following steps: The present application provides a method for preparing a solar cell, characterized by comprising the following steps: S1 provides a silicon substrate, and polishes the front and back sides of the silicon substrate; S2 deposits a tunnel oxide layer and an intrinsic polysilicon layer in sequence along the thickness direction on the back side of the silicon substrate; S3: printing a boron paste according to a pattern on the back side of the intrinsic polysilicon layer away from the silicon substrate by spraying or screen printing, and forming a patterned boron layer after drying. The dried boron layer has a gap region to be doped with n-type; S4: spray-printing or screen-printing phosphorus paste in the gap area of the boron layer according to the pattern, and drying to form a patterned phosphorus layer; S5: performing a boron diffusion doping process and a phosphorus diffusion doping process on the back side of the intrinsic polysilicon layer to form a PN junction on the back side of the intrinsic polysilicon layer; the PN junction includes a first conductive doping structure and a second conductive doping structure arranged in a staggered manner in a finger-like cross-shaped manner, and the back side of the first conductive doping structure away from the silicon substrate forms a borosilicate glass, and the back side of the second conductive doping structure away from the silicon substrate forms a phosphorus silicon glass; S6 performs isolation processing on the first conductive doping structure and the second conductive doping structure to expose the silicon substrate corresponding to the boundary region between the first conductive doping structure and the second conductive doping structure; S7: removing the borosilicate glass on the first conductive doping structure and removing the phosphosilicate glass on the second conductive doping structure; S8 coats the front and back sides of the silicon substrate; S9: printing a metal grid line on the PN junction and sintering the grid line to prepare the solar cell.
[0048] Specifically, the silicon substrate is an N-type silicon wafer.
[0049] In order to remove dirt on the surface of the silicon substrate and surface structural defects when the silicon substrate is cut, this embodiment needs to remove damage, clean and polish the N-type silicon wafer before depositing the tunneling oxide layer and the intrinsic polysilicon layer on the back of the silicon substrate in sequence. This embodiment does not limit the specific method of removing damage, cleaning and polishing, as long as it can ensure that the dirt on the surface of the silicon wafer and the surface structural defects when the silicon wafer is cut can be removed, for example, the N-type silicon wafer can be cleaned with ozone, hydrogen chloride and water; after cleaning, an alkaline solution with a polishing additive is used for polishing.
[0050] Before coating the front and back sides of the silicon substrate, the front side of the silicon substrate needs to be textured to form a pyramid-shaped textured surface on the front side of the silicon substrate to increase light absorption.
[0051] In step S1 of the present application, the front and back sides of the silicon substrate are polished according to the following method: At a temperature of 55-70°C, add 0.2%-1% polishing additive (such as polishing additives of brands such as Shichuang / Tuobang / Sanfeng) to a 2%-8% NaOH aqueous solution and / or a 4-10% KOH aqueous solution, and polish the silicon substrate for 200-300 seconds to prepare a polished surface with a reflectivity of 35-45%.
[0052] Specifically, at a temperature of 60°C, a polishing additive with a volume concentration of 0.4% (such as polishing additives of brands such as Shichuang / Tuobang / Sanfeng) is added to a NaOH aqueous solution with a volume concentration of 5%, and the silicon substrate is polished for 200-300 seconds to prepare a polished surface with a reflectivity of 35-45%.
[0053] This embodiment does not limit the specific method of depositing the tunnel oxide layer (i.e., SiO2 layer) and the intrinsic polysilicon layer, as long as the tunnel oxide layer and the intrinsic polysilicon layer can be formed on the back side of the silicon substrate. In this embodiment, a tunnel oxide layer and an intrinsic polysilicon layer are sequentially deposited along the thickness direction on the back side of the silicon substrate by one of LPCVD, PECVD, and PVD methods, wherein the tunnel oxide layer is composed of SiO2 and has a thickness of 0.8 to 1.6 nm.
[0054] Specifically, when the tunnel oxide layer is deposited by LPCVD, the deposition temperature is 550-750° C., and the deposition time is 10-40 min; when the intrinsic polysilicon layer is deposited by LPCVD, the thickness of the intrinsic polysilicon layer is 50-150 nm, the deposition temperature is 580-680° C., and the deposition time is 30-90 min; When the tunnel oxide layer is deposited by PECVD, the deposition temperature is 350-500°C and the deposition time is 5-30 minutes; when the intrinsic polysilicon layer is deposited by PECVD, the thickness of the intrinsic polysilicon layer is 50-150 nm, the deposition temperature is 350-500°C and the deposition time is 20-70 minutes; When the tunnel oxide layer is deposited by PVD, the deposition temperature is PVD150~300°C and the deposition time is 3~25min; when the intrinsic polysilicon layer is deposited by PVD, the thickness of the intrinsic polysilicon layer is 50~150nm, the deposition temperature is 150~350°C and the deposition time is 5~30min.
[0055] In step S3 of the present application, the boron slurry is composed of a mixture of an organic solvent and boron powder and has a certain rheological property for printing or spraying and other processes. The mass ratio of the boron element in the boron slurry is not less than 10%, the drying temperature is 50~200°C, and the drying time is 1~10min; the phosphorus slurry is composed of a mixture of an organic solvent and phosphorus powder and has a certain rheological property for printing or spraying and other processes. The mass ratio of the phosphorus element in the phosphorus slurry is not less than 10%, the drying temperature is 50~200°C, and the drying time is 1~10min.
[0056] In the present application, the boron paste is first printed on the back side of the intrinsic polysilicon layer away from the silicon substrate by screen printing, and after drying, the phosphorus paste is printed on the gap area to be n-type doped, and the drying process is continued after printing. The following method can also be used: the boron paste and the phosphorus paste are printed on the back side of the intrinsic polysilicon layer away from the silicon substrate by screen printing, and the two printings are uniformly dried at a drying temperature of 50-200°C and a drying time of 1-10 minutes.
[0057] Specifically, in the steps of performing boron diffusion doping treatment and phosphorus diffusion doping treatment on the back side of the intrinsic polysilicon layer, the annealing temperature required for diffusion is controlled at 850-1100°C, and the annealing time is 30-90 minutes. The silicon substrate after forming the intrinsic polysilicon layer is subjected to directional printing of boron source and phosphorus source to form a patterned boron layer and phosphorus layer, and then the boron atoms and phosphorus atoms are doped into the intrinsic polysilicon layer through high-temperature oxygen atmosphere annealing to form a PN junction, wherein the PN junction includes a first conductive doping structure and a second conductive doping structure arranged in an interlaced manner in a finger-like cross-shaped manner, and the back side of the first conductive doping structure away from the silicon substrate forms borosilicate glass, and the back side of the second conductive doping structure away from the silicon substrate forms phosphorus silicon glass.
[0058] In conventional production processes, the back side of the intrinsic polysilicon layer needs to be subjected to boron diffusion doping treatment and phosphorus diffusion doping treatment in steps, which increases the preparation process, increases the production cost, and reduces the production efficiency. The method of the present application improves the boron slurry and the boron slurry, so that when the method prepares solar cells, the intrinsic polysilicon layer on the silicon substrate can be simultaneously subjected to boron diffusion and phosphorus diffusion under the same thermal diffusion conditions without affecting the doping effect, thereby greatly simplifying the process flow and providing the possibility for subsequent large-scale production.
[0059] Specifically, the first conductive doping structure and the second conductive doping structure are isolated to prevent contact leakage between the first conductive doping structure and the second conductive doping structure, thereby affecting battery performance. The specific operation steps are as follows: Laser etching is used to perform etching along the boundary between the first conductive doping structure and the second conductive doping structure until the silicon substrate corresponding to the boundary area between the first conductive doping structure and the second conductive doping structure is exposed, a groove is formed at the boundary between the first conductive doping structure and the second conductive doping structure, and passivation of the groove area is completed in a subsequent process, so that an isolation area is formed at the boundary between the first conductive doping structure and the second conductive doping structure.
[0060] Specifically, before the phosphorus paste is spray-printed or screen-printed in the gap area of the boron layer according to a pattern, a mask layer is formed at the boundary of the gap area in advance by one of the methods of screen printing, inkjet printing, and glue coating, exposure and development.
[0061] Specifically, the isolation treatment step of the first conductive doping structure and the second conductive doping structure is performed according to the following method: The mask layer between the junctions of the first conductive doping structure and the second conductive doping structure is removed, so that an isolation region is formed on the junctions of the first conductive doping structure and the second conductive doping structure.
[0062] It should be noted that, because metal impurities and oxygen impurities are accumulated in the phosphosilicate glass layer and the phosphorus-doped silicon layer, it is necessary to remove the phosphosilicate glass layer and the phosphorus-doped silicon layer. This embodiment does not limit the specific method of removing the phosphosilicate glass layer, as long as the phosphosilicate glass layer can be removed. Specifically, in this application, the steps of removing the borosilicate glass on the first conductive doping structure and removing the phosphosilicate glass on the second conductive doping structure can be performed as follows: The silicon substrate after isolation treatment is cleaned with HF solution with a mass concentration of 15-40% for 1-5 minutes to remove the borosilicate glass and phosphosilicate glass formed on the surface of the silicon substrate after high-temperature annealing, as well as the impurities generated by laser etching isolation.
[0063] Specifically, the steps of coating the front and back sides of the silicon substrate include: A silicon nitride film is deposited on the front side of the silicon substrate by PECVD, the thickness of the silicon nitride film is controlled to be 70-90 nm, and the refractive index is controlled to be between 1.95 and 2.2; A silicon nitride film and an aluminum oxide film are sequentially deposited on the back side of a silicon substrate along a thickness direction by using a PECVD method, wherein the thickness of the silicon nitride film is controlled to be between 70 and 90 nm, and the refractive index is controlled to be between 1.95 and 2.2; the deposition thickness of the aluminum oxide film is controlled to be between 5 and 35 nm.
[0064] Specifically, the steps of printing a metal gate line on the PN junction and performing sintering include: Silver paste grid lines are printed on the PN junction by screen printing, the width of the silver paste grid lines is 20~80μm, and the silver paste grid lines are sintered at 700~850℃.
[0065] The present invention also provides a solar cell, including a solar cell prepared by the method for preparing a solar cell described in the present application.
[0066] Specifically, the solar cell of the present invention comprises: Silicon substrate 1; A tunneling oxide layer 2 formed on the back side of the silicon substrate; An intrinsic polysilicon layer 3 formed on the back side of the tunnel oxide layer 2 away from the silicon substrate; A PN junction 4 is formed on the back side of the intrinsic polysilicon layer 3 away from the silicon substrate; the PN junction 4 includes a first conductive doping structure 41 and a second conductive doping structure 42 which are arranged in a staggered manner in a finger-like cross-shaped manner, and an isolation region is provided between the first conductive doping structure 41 and the second conductive doping structure 42; A first passivation anti-reflection layer 5 formed on the front side of the silicon substrate; A second passivation anti-reflection layer 6 formed on the back side of the silicon substrate; and / or A metal gate line 7 is formed on the PN junction.
[0067] Specifically, the silicon substrate is an N-type silicon wafer.
[0068] Specifically, the thickness of the tunnel oxide layer is 0.8-1.6 nm.
[0069] Specifically, the thickness of the tunnel oxide layer is 1.2 nm.
[0070] Specifically, the thickness of the intrinsic polysilicon layer is 120 nm.
[0071] Specifically, the first passivation anti-reflection layer is a silicon nitride film deposited on the front side of the silicon substrate by PECVD, the thickness of the silicon nitride film is controlled to be 70-90 nm, and the refractive index is controlled to be between 1.95 and 2.2.
[0072] Specifically, a pyramid velvet surface is formed between the front surface of the silicon substrate and the first passivation anti-reflection layer, and the reflectivity of the pyramid velvet surface is 9-12%.
[0073] Specifically, the second passivation anti-reflection layer includes a silicon nitride film 61 and an aluminum oxide film 62 deposited in sequence along the thickness direction of the silicon substrate, wherein the thickness of the silicon nitride film is controlled to be 70-90 nm, and the refractive index is controlled to be between 1.95 and 2.2; the deposition thickness of the aluminum oxide film is controlled to be between 5 and 35 nm.
[0074] The performance of the solar cell prepared by the method of the present application was compared with that of the cell prepared by the conventional process. The test results are shown in Table 1.
[0075] Table 1 Quantity / piece Opening voltage VOC / mV Short Flow ISC / A Fill Factor FF Efficiency Yield Control group (conventional process) 500 745.3 13.96 84.33% 26.49% 97.1% Experimental group 500 745.6 13.98 84.26% 26.51% 97.4% As can be seen from Table 1, this method reduces product defects such as fragmentation rate and scratches by more than 0.2% while ensuring product yield, and reduces the process flow by more than 3 steps; the photovoltaic efficiency yield is 0.1%, which is very high, with a daily production capacity of one million pieces.
[0076] The above examples are for the purpose of illustrating the embodiments disclosed in the present application and should not be construed as limiting the present application. In addition, the various modifications listed herein and the changes in the methods and compositions in the application are obvious to those skilled in the art without departing from the scope and spirit of the present application. Although the present application has been specifically described in conjunction with a variety of specific preferred embodiments of the present application, it should be understood that the present application should not be limited to these specific embodiments. In fact, various modifications as described above that are obvious to those skilled in the art to obtain the application should be included in the scope of the present application.
Claims
1. A method for preparing a solar cell, characterized in that: The following steps are involved: Providing a silicon substrate, and polishing the front and back sides of the silicon substrate; Depositing a tunnel oxide layer and an intrinsic polysilicon layer in sequence along the thickness direction on the back side of the silicon substrate; Boron slurry is spray-printed or screen-printed according to a pattern on the back side of the intrinsic polysilicon layer away from the silicon substrate, and a patterned boron layer is formed after drying, wherein the dried boron layer has a gap region to be doped with n-type; In the gap area of the boron layer, phosphorus paste is spray-printed or screen-printed according to a pattern, and dried to form a patterned phosphorus layer; The back side of the intrinsic polysilicon layer is subjected to boron diffusion doping treatment and phosphorus diffusion doping treatment to form a PN junction on the back side of the intrinsic polysilicon layer; the PN junction includes a first conductive doping structure and a second conductive doping structure arranged in a staggered manner in a finger-like cross-shaped manner, and the back side of the first conductive doping structure away from the silicon substrate forms borosilicate glass, and the back side of the second conductive doping structure away from the silicon substrate forms phosphorus silicon glass; Isolating the first conductive doping structure and the second conductive doping structure to expose the silicon substrate corresponding to the boundary region between the first conductive doping structure and the second conductive doping structure; removing the borosilicate glass on the first conductive doping structure, and removing the phosphosilicate glass on the second conductive doping structure; Coating the front and back sides of a silicon substrate; The metal grid line is printed on the PN junction and sintered to prepare the solar cell.
2. The method for preparing a solar cell according to claim 1, characterized in that: The silicon substrate is an N-type silicon wafer.
3. The method for preparing a solar cell according to claim 1, characterized in that: The steps of polishing the front and back sides of the silicon substrate are performed as follows: At a temperature of 55-70°C, a polishing additive with a volume concentration of 0.2%-1% is added to a 2%-8% NaOH aqueous solution or a 4-10% KOH aqueous solution to polish a silicon substrate for 200-300 seconds to prepare a polished surface with a reflectivity of 35-45%.
4. The method for preparing a solar cell according to claim 1, characterized in that: Depositing a tunnel oxide layer and an intrinsic polysilicon layer in sequence along the thickness direction on the back side of the silicon substrate by one of LPCVD, PECVD and PVD, wherein the tunnel oxide layer is composed of SiO2 and has a thickness of 0.8-1.6 nm; When the tunnel oxide layer is deposited by LPCVD, the deposition temperature is 550-750° C., and the deposition time is 10-40 min. When the intrinsic polysilicon layer is deposited by LPCVD, the thickness of the intrinsic polysilicon layer is 50-150 nm, the deposition temperature is 580-680° C., and the deposition time is 30-90 min. When the tunnel oxide layer is deposited by PECVD, the deposition temperature is 350-500°C and the deposition time is 5-30 minutes; when the intrinsic polysilicon layer is deposited by PECVD, the thickness of the intrinsic polysilicon layer is 50-150 nm, the deposition temperature is 350-500°C and the deposition time is 20-70 minutes; When the tunnel oxide layer is deposited by PVD, the deposition temperature is PVD150~300°C and the deposition time is 3~25min; when the intrinsic polysilicon layer is deposited by PVD, the thickness of the intrinsic polysilicon layer is 50~150nm, the deposition temperature is 150~350°C and the deposition time is 5~30min.
5. The method for preparing a solar cell according to claim 1, characterized in that: The boron slurry is composed of a mixture of an organic solvent and boron powder and has a certain rheological property for printing or spraying. The mass ratio of the boron element in the boron slurry is not less than 10%, the drying temperature is 50~200℃, and the drying time is 1~10min; the phosphorus slurry is composed of a mixture of an organic solvent and phosphorus powder and has a certain rheological property for printing or spraying. The mass ratio of the phosphorus element in the phosphorus slurry is not less than 10%, the drying temperature is 50~200℃, and the drying time is 1~10min.
6. The method for preparing a solar cell according to claim 1, characterized in that: In the steps of performing boron diffusion doping treatment and phosphorus diffusion doping treatment on the back side of the intrinsic polysilicon layer, the annealing temperature required for diffusion is controlled at 850-1100° C., and the annealing time is 30-90 minutes.
7. The method for preparing a solar cell according to claim 6, characterized in that: In the steps of performing boron diffusion doping treatment and phosphorus diffusion doping treatment on the back side of the intrinsic polysilicon layer, the annealing temperature required for diffusion is controlled at 850-1050°C.
8. The method for preparing a solar cell according to claim 1, characterized in that: Before the phosphorus paste is spray-printed or screen-printed in the gap area of the boron layer according to the pattern, a mask layer is formed at the junction of the gap area by screen printing, inkjet printing, glue coating, exposure and development.
9. The method for preparing a solar cell according to claim 1, characterized in that: The isolation treatment steps for the first conductive doping structure and the second conductive doping structure are performed as follows: Laser etching is used to perform etching along the boundary between the first conductive doping structure and the second conductive doping structure until the silicon substrate corresponding to the boundary area between the first conductive doping structure and the second conductive doping structure is exposed, a groove is formed at the boundary between the first conductive doping structure and the second conductive doping structure, and passivation of the groove area is completed in a subsequent process, so that an isolation area is formed at the boundary between the first conductive doping structure and the second conductive doping structure.
10. A solar cell, characterized in that: A solar cell prepared by the method for preparing a solar cell according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of IBC solar cell with passivation contact structure, cell, assembly and system
CN115274913A
Preparation method of novel full back electrode passivation contact cell and product thereof
CN116130558A
Method for preparing TBC battery
CN116936677A
Back contact solar cell and preparation method thereof
CN118248783A