Slice battery edge isolation method and slice battery

The nanosecond laser combined with wet etching process forms an isolation area at the edge of the sliced ​​battery, suppressing carrier recombination, solving the problems of sliced ​​battery efficiency loss and high production cost, and achieving efficient and low-cost battery performance improvement.

CN119029092APending Publication Date: 2024-11-26CHINA SCI & TECH (NINGBO) CO LTD
View PDF 0 Cites 7 Cited by

Patent Information

Application Number
CN202411136744.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Edge recombination generated by sliced ​​batteries during cutting results in loss of efficiency. Prior art such as alumina edge passivation methods are costly and inefficient, affecting the appearance of the battery.

Method used

Using nanosecond laser combined with wet etching technology, an isolation area without pn junction is formed between the cutting edge of the sliced ​​battery and the metal electrode, inhibiting carrier recombination, and removing the damaged layer by pickling and alkali washing, and preparing AlOx and SiNx Laminated thin film passivation layer to reduce battery efficiency loss.

Benefits of technology

It significantly reduces battery efficiency loss, achieves battery performance without leakage, low saturation current density and high filling factor, while reducing production costs, and is suitable for different types of sliced ​​batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029092A_ABST
    Figure CN119029092A_ABST
Patent Text Reader

Abstract

According to the slice battery edge isolation method and the slice battery provided by the invention, nanosecond laser is combined with a wet etching process, an isolation region without a pn junction is formed between the cutting edge of the slice battery and a metal electrode, and the isolation region can cut off a transmission channel of minority carriers from a battery working region to a cutting part; and the influence of minority carrier recombination dark current at the cutting part on the working area of the battery is inhibited, so that the effect of improving the efficiency of the sliced battery is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of crystalline silicon solar cell preparation, and in particular to a sliced ​​cell edge isolation method and a sliced ​​cell. Background Art

[0002] Slicing technology refers to cutting a single cell into the same half or multiple cells, and then welding the sliced ​​cells in series. This technology has the effects of improving packaging efficiency, reducing component temperature rise, and reducing shading losses. However, cutting cells will inevitably cause laser thermal ablation and mechanical damage, and defects on the surface or edge of the cell will cause carriers (electrons and holes) to recombine at the edges of these defects. For tunneling oxide silicon passivated contact (TOPCon) sliced ​​cells, the efficiency impact caused by edge recombination will be very significant, and the efficiency loss will reach 0.2% to 0.4%.

[0003] In order to deal with the efficiency loss caused by the slicing process, the industry has proposed to use atomic layer deposition (ALD) technology to deposit a certain thickness (about 30nm) of aluminum oxide (AlO) on the edge of the silicon wafer after the battery is sliced. x ) to passivate the edges, which can increase the efficiency of existing sliced ​​cells by 0.1% to 0.2%. However, the production cost of this technology is high, the production efficiency is low, the cost performance of industrial application is low, and the aluminum oxide will be plated around the battery, affecting the appearance of the battery. Summary of the invention

[0004] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is how to improve the efficiency of sliced ​​batteries, reduce production costs, and meet the needs of industrial applications.

[0005] To achieve the above object, the present invention provides a first aspect of a cell edge isolation method, comprising the following steps:

[0006] a. Prepare a passivation sheet, the passivation sheet includes a silicon wafer, a boron emitter and borosilicate glass are sequentially arranged on the front side of the silicon wafer, and a nano silicon oxide layer and a phosphorus-doped polysilicon layer are sequentially arranged on the back side of the silicon wafer;

[0007] b. Use nanosecond laser to etch holes on the front of the silicon wafer to remove the borosilicate glass and part of the boron emitter to form an isolation area;

[0008] c. The isolation area is acid-washed and alkaline-washed in sequence to remove the residual borosilicate glass and boron emitter in the isolation area and form a new surface structure;

[0009] d. Etching to remove the borosilicate glass from the remaining area on the front side of the silicon wafer;

[0010] e. preparing a front passivation layer and a back passivation layer on the front and back of the passivation sheet respectively;

[0011] f. Double-sided metallization of the passivation sheet;

[0012] g. Perform laser non-destructive cutting, with the cutting part in the isolation area or on one side of the isolation area, and a cutting area is formed on the side of the silicon wafer. The present invention uses nanosecond laser combined with wet etching process to form an isolation area without pn junction between the cutting edge of the sliced ​​battery and the metal electrode. The isolation area can cut off the transmission channel of minority carriers from the battery working area to the cutting part, inhibit the influence of the minority carrier recombination dark current in the cutting part on the battery working area, thereby achieving the effect of improving the efficiency of the sliced ​​battery.

[0013] Furthermore, in step b, the wavelength of the nanosecond laser is 500-1100 nm. The use of nanosecond laser for etching the opening of the boron emitter has low equipment investment cost and is conducive to industrial application.

[0014] Furthermore, in step b, the laser pulse energy density is >0.3 J / cm 2 The spot overlap rate is 5% to 90%, and the pulse width is 1 to 500ns. By controlling the process parameters of nanosecond laser, the boron emitter in the isolation area can be etched cleanly to avoid boron emitter residue and improve the isolation effect.

[0015] Furthermore, in step S30, after the isolation area is pickled and alkali washed, the surface structure of the isolation area is a velvet surface or a flat structure. The isolation area forms a new surface structure, achieving good surface passivation without generating additional composites.

[0016] Furthermore, in step c, a hydrofluoric acid solution is used for pickling to remove the borosilicate glass, and an alkali solution is used for alkali washing to remove the boron emitter. The appropriate etching solution is controlled and selected to ensure the etching effect, while avoiding excessive etching to cause surface defects. Furthermore, in step b, the width of the isolation zone formed by the nanosecond laser opening is greater than 10 μm. The isolation zone has a certain width to ensure the isolation effect.

[0017] Furthermore, in step f, the distance between the cutting part and the isolation area is less than 10 mm. The isolation area and the cutting part are arranged close to each other to improve the isolation effect.

[0018] Furthermore, the cell edge isolation method further comprises the steps of:

[0019] g. Use alkali solution to etch the cutting area to remove the damaged layer;

[0020] h. Prepare a side passivation layer on the cutting area.

[0021] The cut area is alkaline etched and passivated to reduce its surface recombination, thereby reducing the loss of battery efficiency.

[0022] Furthermore, in step h, the side passivation layer prepared is AlO x With SiN x Laminated film. This passivation layer can make the cutting area have good surface passivation without generating additional recombination.

[0023] The first aspect of the present invention provides a sliced ​​battery, which is prepared by the above-mentioned sliced ​​battery edge isolation method. The sliced ​​battery of the present invention has the advantages of no leakage, low saturation current density, high filling factor, high battery efficiency, etc.

[0024] In summary, the present invention has the following beneficial effects compared with the prior art:

[0025] (1) The present invention forms an isolation area on the battery surface by combining nanosecond laser with wet etching process, cuts off the transmission channel of minority carriers from the battery working area to the cutting part, suppresses significant carrier recombination in the cutting area, and thus reduces battery efficiency loss.

[0026] (2) The method of the present invention sequentially performs acid washing and alkali washing on the isolation area, which can effectively remove the damage caused by the nanosecond laser, and through the subsequent deposition of a passivation layer, the isolation area can achieve good surface passivation without generating additional recombination.

[0027] (3) The sliced ​​battery prepared by the method of the present invention has no wrap-around plating, no appearance color difference, the isolation area is covered with a passivation film, and there is no obvious laser cutting mark.

[0028] (4) The method of the present invention performs alkaline etching and passivation on the cut area to reduce its surface recombination, thereby reducing the loss of battery efficiency.

[0029] (5) The method of the present invention is simple to implement and is fully compatible with existing production line processes. It only requires the addition of one or two nanosecond lasers, without changing the existing battery process. The equipment cost is low and the production line can be easily modified. This method can be applied to sliced ​​batteries of different types such as one-cut two, one-cut three, and one-cut multiple. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a flow chart of the cell edge isolation method of sliced ​​cells in a specific embodiment of the present invention.

[0031] Figure 2 It is a schematic diagram of the structural changes during the process of the cell edge isolation method in a specific embodiment of the present invention.

[0032] Figure 3 It is a schematic diagram of the structure of a sliced ​​battery with edge isolation in a specific implementation manner of the present invention.

[0033] Figure 4 This is a morphology diagram of the boron emitter with borosilicate glass in Example 1 of the present invention.

[0034] Figure 5 This is a morphology diagram of the isolation area after nanosecond laser hole opening and etching in Example 3 of the present invention.

[0035] Figure 6 This is a morphology diagram of the isolation area after pickling in Example 3 of the present invention.

[0036] Figure 7 This is a morphology diagram of the isolation area after alkali washing in Example 3 of the present invention.

[0037] Figure 8 This is an ECV curve diagram of the isolation zone in Example 3 of the present invention.

[0038] Fig. 9 This is a morphology diagram of the isolation area after alkali washing in Example 5 of the present invention.

[0039] Fig.10 This is an ECV curve diagram of the isolation zone in Example 6 of the present invention.

[0040] Fig.11 The topography of the isolation area obtained by processing the four light spot overlap ratios in Example 9 of the present invention.

[0041] Fig.12 This is the ECV curve diagram of the laser processed area in Comparative Example 4.

[0042] Description of reference numerals:

[0043] 1-silicon wafer, 2-boron emitter, 3-isolation area, 4-nano silicon oxide layer, 5-phosphorus-doped polysilicon layer, 6-front passivation layer, 7-front electrode, 8-back passivation layer, 9-back electrode, 10-cutting area, 11-phosphorus diffusion layer. DETAILED DESCRIPTION

[0044] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. It should be noted that the following embodiments are only used to illustrate the implementation method and typical parameters of the present invention, and are not used to limit the parameter range described in the present invention. Reasonable changes derived therefrom are still within the scope of protection of the claims of the present invention.

[0045] It should be noted that the endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.

[0046] The specific embodiment of the present invention provides a method for isolating the edge of a sliced ​​battery, combining Figure 1 and Figure 2 As shown, the following steps are included:

[0047] (1) A passivation wafer is prepared. The passivation wafer comprises a silicon wafer 1. A boron emitter 2 and borosilicate glass are sequentially arranged on the front side of the silicon wafer 1. A nano silicon oxide layer 4 and a phosphorus-doped polysilicon layer 5 are sequentially arranged on the back side of the silicon wafer 1.

[0048] (2) Use nanosecond laser to open holes on the front side of the silicon wafer 1, remove the borosilicate glass and part of the boron emitter 2, and form an isolation region 3. In a specific embodiment, this step can use a nanosecond laser with a wavelength of 500 to 1100 nm for surface treatment, and the laser parameters are as follows: the laser pulse energy density is >0.3 J / cm 2 , the spot overlap rate is 5% to 90%, and the pulse width is 1 to 500ns. Preferably, the width of the isolation area 3 formed by the nanosecond laser opening is greater than 10 μm to ensure the isolation effect.

[0049] (3) The isolation area 3 is pickled to remove the residual borosilicate glass in the isolation area 3. In a specific embodiment, the pickling liquid is a hydrofluoric acid solution.

[0050] (4) Alkaline washing is performed on the isolation region 3 to remove the residual boron emitter 2 in the isolation region 3 and form a new surface structure. In a specific embodiment, alkaline washing is performed with an alkaline solution, such as a sodium hydroxide solution, a potassium hydroxide solution, a TMAH solution, etc. After this step, the passivation sheet structure is as follows: Figure 2 As shown. Due to the long pulse width of nano-laser, it produces a strong interaction and thermal effect with the surface in the laser irradiation area, which can significantly destroy the surface borosilicate glass and pyramid velvet structure; after the borosilicate glass is removed by acid washing, a new plane or velvet structure is formed in the subsequent alkaline washing stage. The new surface structure is mainly affected by the laser parameters.

[0051] (5) Etching to remove the borosilicate glass in the remaining area on the front side of the silicon wafer 1.

[0052] (6) A front passivation layer 6 and a back passivation layer 8 are prepared on the front and back sides of the passivation sheet, respectively.

[0053] (7) The passivation film is metallized on both sides.

[0054] (8) Laser non-destructive cutting is performed, and the cutting part is in the isolation area 3 or away from the electrode side. In a preferred embodiment, the distance between the cutting part and the isolation area 3 is less than 10 mm to ensure the isolation effect. After laser non-destructive cutting, a cutting area 10 is formed on the side of the silicon wafer 1.

[0055] (9) Use alkaline solution to etch the cutting area 10 to remove the damaged layer.

[0056] (10) Prepare a side passivation layer on the cutting area 10, and the side passivation layer is preferably AlO x With SiN x Laminated film.

[0057] Combination Figure 3 As shown, the typical structure of the sliced ​​battery prepared by the above method is as follows: the sliced ​​battery includes a silicon wafer 1, and the side of the silicon wafer 1 has a cutting area 10 formed by laser non-destructive cutting; the surface of the cutting area 10 is covered with a side passivation layer (not shown in the figure). The front side of the silicon wafer 1 has a boron emitter 2, forming a battery working area; a front passivation layer 6 is provided on the boron emitter 2; and a front electrode 7 in contact with the boron emitter 2 is also provided on the front side of the silicon wafer 1. All boron emitters 2 are removed from the front side of the silicon wafer 1 near the cutting area 10 to form an isolation area 3, which can cut off the transmission channel of minority carriers from the battery working area to the cutting area 10. The surface morphology of the isolation area 3 is flat ( Figure 3 Middle A) or suede ( Figure 3 B), and different from the surface structure of the silicon wafer 1, the front passivation layer 6 covers the isolation region 3, and the composite current density of this region after passivation is low. The back of the silicon wafer 1 has a phosphorus diffusion layer 11, and the phosphorus diffusion layer 11 is provided with a nano silicon oxide layer 4 and a phosphorus-doped polysilicon layer 5; the phosphorus-doped polysilicon layer 5 is provided with a back passivation layer 8; the back of the silicon wafer 1 is also provided with a back electrode 9 in contact with the phosphorus-doped polysilicon layer 8.

[0058] The above method uses nanosecond laser combined with wet etching to form an isolation area without pn junction between the cutting area and the electrode, thereby suppressing significant carrier recombination in the cutting area and preventing the recombination center from injecting recombination dark current into the battery working area through the minority carrier channel of the pn junction, thereby reducing battery efficiency loss.

[0059] The technical solutions and effects of the present invention are illustrated below through specific embodiments.

[0060] Example 1

[0061] The steps for preparing the TOPCon structure passivation wafer are as follows: prepare n-type silicon wafers, perform front texturing, back polishing, and standard RCA cleaning. Boron is diffused on the front of the silicon wafer to form a boron emitter; the back is polished to remove the borosilicate glass. Nano silicon oxide and phosphorus-doped amorphous silicon are deposited on the back in sequence. Annealing treatment is performed at 900℃ for 30 minutes to obtain the TOPCon structure passivation wafer. The surface morphology of the boron emitter with borosilicate glass on the front of the cell is observed, and the results are as follows: Figure 4 As shown, the conductivity type of the boron emitter is measured to be P type.

[0062] Example 2

[0063] The steps of preparing a TOPCon whole cell are as follows: prepare the TOPCon structure passivation sheet obtained in Example 1, and remove the borosilicate glass by etching on the front side. Prepare an aluminum oxide film on the front side of the sample, and then deposit a silicon nitride film on both sides. Metallize the sample on both sides to obtain a TOPCon whole cell.

[0064] Test the performance of the prepared whole battery, open circuit voltage (V oc ) is 735mV, the short-circuit current density (J sc ) is 41.81 mA / cm 2 , the fill factor (FF) is 85.68% and the cell efficiency (Eff) is 25.94%.

[0065] Example 3

[0066] The edge-isolated TOPCon sliced ​​cells are prepared in the following steps: the front side of the TOPCon structure sample obtained in Example 1 is treated with a nanosecond laser with a wavelength of 550 nm, and the laser pulse energy density is 1 J / cm 2 The spot overlap rate is 10%, the pulse width is 50ns, most of the borosilicate glass and part of the boron emitter are removed to form an isolation area. The width of this area is 80μm, and its surface morphology is as follows Figure 5 The isolation area is pickled with hydrofluoric acid solution to remove the residual borosilicate glass. The surface morphology is shown in Figure 6 The isolation area is alkaline washed with sodium hydroxide solution to remove the residual boron emitter. The surface morphology is shown in Figure 7 As shown in Figure 1, a planar structure is formed. The ECV curve of the isolation area is tested and the results are shown in Figure 1. Figure 8 As shown, the blue dotted line represents electrons, indicating that the boron emitter has been removed and the conductivity type is N-type. The borosilicate glass in the remaining area on the front of the sample is etched away. Aluminum oxide film is prepared on the front of the sample, and then silicon nitride film is deposited on both sides. The passivation film is metallized on both sides. Laser non-destructive cutting is performed on the isolation area to obtain a sliced ​​battery with edge isolation.

[0067] Test the performance of the prepared slice battery, V oc is 733mV, J sc 41.80mA / cm 2 , FF is 85.65%, and Eff is 25.87%.

[0068] Example 4

[0069] The edge-isolated TOPCon sliced ​​cells are prepared in the following steps: the front side of the TOPCon structure sample obtained in Example 1 is treated with a nanosecond laser with a wavelength of 550 nm, and the laser pulse energy density is 1 J / cm 2, the spot overlap rate is 10%, the pulse width is 50ns, and an isolation area is formed with an isolation area width of 80μm. The isolation area is pickled with hydrofluoric acid solution to remove the residual borosilicate glass. The isolation area is alkaline washed with sodium hydroxide solution to remove the residual boron emitter, and the surface of the isolation area is a planar structure. The conductivity type of the tested isolation area is N-type. Etch to remove the borosilicate glass in the remaining area on the front of the sample. Prepare an aluminum oxide film on the front of the sample, and then deposit a silicon nitride film on the front and back. The sample is double-sided metallized. Align the isolation area for laser non-destructive cutting to obtain an edge-isolated sliced ​​sample. Etch the cutting area with sodium hydroxide solution, and then deposit an aluminum oxide film and a silicon nitride film on the surface of the cutting area to obtain an edge-isolated sliced ​​battery.

[0070] Test the performance of the prepared slice battery, V oc is 734mV, J sc 41.81mA / cm 2 , FF is 85.67%, and Eff is 25.91%.

[0071] Example 5

[0072] The edge-isolated TOPCon sliced ​​cells were prepared in the following steps: the front side of the TOPCon structure sample obtained in Example 1 was treated with a nanosecond laser with a wavelength of 520 nm, and the laser pulse energy density was 10 J / cm 2 The spot overlap rate is 60%, the pulse width is 10ns, most of the borosilicate glass and part of the boron emitter are removed to form an isolation area with a width of 60μm. The isolation area is pickled with hydrofluoric acid solution to remove the residual borosilicate glass. The isolation area is alkaline washed with sodium hydroxide solution to remove the residual boron emitter. The surface morphology is as follows Fig. 9 As shown, a new velvet structure is formed. The conductivity type of the test isolation area is N-type. The borosilicate glass in the remaining area of ​​the front side of the sample is removed by etching. Aluminum oxide film is prepared on the front side of the sample, and then silicon nitride film is deposited on both sides. The passivation film is metallized on both sides. Laser non-destructive cutting is performed on the isolation area to obtain a sliced ​​battery with edge isolation.

[0073] Test the performance of the prepared slice battery, V oc is 734mV, J sc 41.80mA / cm 2 , FF is 85.66%, and Eff is 25.89%.

[0074] Example 6

[0075] The edge-isolated TOPCon sliced ​​cells were prepared in the following steps: the front side of the TOPCon structure sample obtained in Example 1 was treated with a nanosecond laser with a wavelength of 900 nm, and the laser pulse energy density was 0.5 J / cm2 The spot overlap rate is 5%, the pulse width is 100ns, most of the borosilicate glass and part of the boron emitter are removed to form an isolation area with a width of 80μm. The isolation area is pickled with hydrofluoric acid solution to remove the residual borosilicate glass. The isolation area is alkaline washed with sodium hydroxide solution to remove the residual boron emitter. The surface of the isolation area is a planar structure. The ECV curve of the isolation area is tested, and the results are as follows Fig.10 As shown, the blue dotted line represents electrons, indicating that the boron emitter has been removed and the conductivity type is N-type. The borosilicate glass in the remaining area on the front side of the sample is etched away. An aluminum oxide film is prepared on the front side of the sample, and then a silicon nitride film is deposited on the front and back sides. The sample is double-sided metallized. Laser non-destructive cutting is performed at a distance of 5 mm from the isolation area to obtain a sliced ​​cell with edge isolation.

[0076] Test the performance of the prepared slice battery, V oc is 733mV, J sc 41.80mA / cm 2 , FF is 84.65%, and Eff is 25.87%.

[0077] Example 7

[0078] The edge-isolated TOPCon sliced ​​cells were prepared in the following steps: the front side of the TOPCon structure sample obtained in Example 1 was treated with a nanosecond laser with a wavelength of 900 nm, and the laser pulse energy density was 20 J / cm 2 , the spot overlap rate is 70%, the pulse width is 80ns, most of the borosilicate glass and part of the boron emitter are removed to form an isolation area with a width of 100μm. The isolation area is pickled with hydrofluoric acid solution to remove the residual borosilicate glass. The isolation area is alkaline washed with sodium hydroxide solution to remove the residual boron emitter, and the surface of the isolation area is a new velvet structure. The conductivity type of the tested isolation area is N-type. Etch to remove the borosilicate glass in the remaining area on the front of the sample. An aluminum oxide film is prepared on the front of the sample, and then a silicon nitride film is deposited on the front and back. The sample is double-sided metallized. Laser non-destructive cutting is performed at a distance of 5mm from the isolation area to obtain an edge-isolated sliced ​​battery.

[0079] Test the performance of the prepared slice battery, V oc is 734mV, J sc 41.80mA / cm 2 , FF is 84.65%, and Eff is 25.88%.

[0080] Example 8

[0081] The edge-isolated TOPCon sliced ​​cells were prepared in the following steps: two locations on the front side of the TOPCon structure sample obtained in Example 1 were treated with a nanosecond laser having a wavelength of 1000 nm, and the laser pulse energy density was 15 J / cm 2 , the spot overlap rate is 20%, the pulse width is 3ns, most of the borosilicate glass and part of the boron emitter are removed to form two isolation areas, and the width of the two isolation areas is 60μm. The cutting area is etched with sodium hydroxide solution to remove the damaged layer. The isolation area is pickled with hydrofluoric acid solution to remove the residual borosilicate glass. The isolation area is alkaline washed with sodium hydroxide solution to remove the residual boron emitter, and the surface of the isolation area is a planar structure. The conductivity type of the test isolation area is N-type. Etch to remove the borosilicate glass in the remaining area of ​​the front of the sample. Prepare an aluminum oxide film on the front of the sample, and then deposit a silicon nitride film on the front and back. The sample is double-sided metallized. Align the two isolation areas for laser non-destructive cutting to obtain 3 sliced ​​samples. Select a sample with cutting areas on both sides, etch the cutting area with sodium hydroxide solution, and then deposit an aluminum oxide film and a silicon nitride film on the surface of the cutting area to obtain an edge-isolated sliced ​​battery.

[0082] Test the performance of sliced ​​cells with cutting areas on both sides, V oc is 734mV, J sc 41.81mA / cm 2 , FF is 84.66%, and Eff is 25.89%.

[0083] Example 9

[0084] The surface morphology is characterized by the following steps: the front side of the four TOPCon structure samples obtained in Example 1 is treated with a nanosecond laser with a wavelength of 520 nm, and the laser pulse energy density is 3 J / cm 2 The spot overlap rate is 50%, 60%, 70%, and 80% respectively, and the pulse width is 100ns. Most of the borosilicate glass and part of the boron emitter are removed to form an isolation area. The isolation area is pickled with hydrofluoric acid solution to remove the residual borosilicate glass. The isolation area is alkaline washed with potassium hydroxide solution to remove the residual boron emitter. The morphology of the isolation area of ​​the four samples is observed, and the results are as follows Fig.11 As shown, in the figure, a corresponds to the sample with a spot overlap rate of 50%, b corresponds to the sample with a spot overlap rate of 60%, c corresponds to the sample with a spot overlap rate of 70%, and d corresponds to the sample with a spot overlap rate of 80%. It can be seen that the surface pyramid velvet results have significant differences.

[0085] Comparative Example 1

[0086] The steps of preparing a TOPCon sliced ​​cell are as follows: prepare the TOPCon structure sample prepared in Example 1, and remove the borosilicate glass on the front side of the sample by etching. Prepare an aluminum oxide film on the front side of the sample, and then deposit a silicon nitride film on both sides. Metallize both sides of the sample. Perform laser non-destructive cutting to obtain a sliced ​​cell.

[0087] Test the performance of the prepared slice battery, V oc is 728mV, J sc 41.79 mA / cm 2 , FF is 85.02%, and Eff is 25.59%.

[0088] Comparative Example 2

[0089] The steps of preparing a TOPCon sliced ​​cell are as follows: prepare the TOPCon structure sample prepared in Example 1, and remove the borosilicate glass on the front side of the sample by etching. Prepare an aluminum oxide film on the front side of the sample, and then deposit a silicon nitride film on both sides. Metallize the sample on both sides. Perform laser non-destructive cutting to obtain a sliced ​​cell. Use ALD to deposit aluminum oxide with a certain thickness of 30nm in the cutting area.

[0090] Test the performance of the prepared slice battery, V oc is 731mV, J sc 41.80mA / cm 2 , FF is 85.25%, and Eff is 25.69%.

[0091] Comparative Example 3

[0092] The steps of preparing a TOPCon sliced ​​cell are as follows: prepare the TOPCon structure sample prepared in Example 1, and remove the borosilicate glass on the front of the TOPCon cell by etching. Prepare an aluminum oxide film on the front of the sample, and then deposit a silicon nitride film on both sides. Metallize the sample on both sides. Perform laser non-destructive cutting on two parts, and divide the cell into three sliced ​​cells, one of which has cutting areas on both sides.

[0093] Test the performance of sliced ​​cells with cutting areas on both sides, V oc is 729mV, J sc 41.79 mA / cm 2 , FF is 83.01%, and Eff is 25.58%.

[0094] Comparative Example 4

[0095] The steps for preparing TOPCon sliced ​​cells are as follows: Use a nanosecond laser with a wavelength of 550nm to treat the front of the TOPCon structure sample obtained in Example 1, and only remove a small part of the borosilicate glass and the boron emitter. The treated area is the laser treated area, and the width of this area is 80μm. Use hydrofluoric acid solution to pickle the laser treated area to remove the residual borosilicate glass. Use sodium hydroxide solution to alkaline wash the laser treated area, and still retain a part of the borosilicate glass and a certain thickness of the boron emitter, and its surface is a velvet structure. Test the ECV curve of the laser treated area, and the results are as follows: Fig.12 As shown, the blue dotted line represents electrons, the red dotted line represents holes, and the boron emitter exists, and the conductivity type is P type. The borosilicate glass in the remaining area of ​​the front side of the sample is removed by etching. Aluminum oxide film is prepared on the front side of the sample, and then silicon nitride film is deposited on both sides. The passivation film is metallized on both sides. Laser non-destructive cutting is performed on the isolation area to obtain a sliced ​​battery with edge isolation.

[0096] Test the performance of sliced ​​cells with cutting areas on both sides, V oc 730mV, J sc 41.79 mA / cm 2 , FF is 83.10%, and Eff is 25.65%.

[0097] The TOPCon battery performances of Examples 2-8 and Comparative Examples 1-4 are shown in Table 1 below.

[0098] Table 1 Comparison of battery performance between examples and comparative examples

[0099] sample <![CDATA[V oc (mV)]]> <![CDATA[J sc (mA / cm 2 )]]> FF(%) Eff(%) Example 2 735 41.81 85.68 25.94 Example 3 733 41.80 85.65 25.87 Example 4 734 41.81 85.67 25.91 Example 5 734 41.80 85.66 25.89 Example 6 733 41.80 85.65 25.87 Example 7 734 41.80 85.65 25.88 Example 8 734 41.81 84.66 25.89 Comparative Example 1 728 41.79 85.02 25.59 Comparative Example 2 731 41.80 85.25 25.69 Comparative Example 3 729 41.79 83.01 25.58 Comparative Example 4 730 41.79 83.10 25.65

[0100] Test results show that the efficiency of cells that have undergone laser edge isolation is about 0.3% higher than that of directly sliced ​​cells, significantly reducing the efficiency loss of sliced ​​cell pairs. The operation is simple and will not affect the appearance of the cell, making it suitable for industrial promotion and application.

[0101] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for isolating the edge of a sliced ​​battery, characterized in that: The following steps are involved: a. Prepare a passivation sheet, the passivation sheet includes a silicon wafer, a boron emitter and borosilicate glass are sequentially arranged on the front side of the silicon wafer, and a nano silicon oxide layer and a phosphorus-doped polysilicon layer are sequentially arranged on the back side of the silicon wafer; b. Use nanosecond laser to etch holes on the front of the silicon wafer to remove the borosilicate glass and part of the boron emitter to form an isolation area; c. The isolation area is acid-washed and alkaline-washed in sequence to remove the residual borosilicate glass and boron emitter in the isolation area and form a new surface structure; d. Etching to remove the borosilicate glass from the remaining area on the front side of the silicon wafer; e. preparing a front passivation layer and a back passivation layer on the front and back of the passivation sheet respectively; f. Double-sided metallization of the passivation sheet; g. Perform laser non-destructive cutting, with the cutting area being inside the isolation area or on one side of the isolation area, and a cutting area being formed on the side of the silicon wafer.

2. The cell edge isolation method according to claim 1, characterized in that: In the step b, the wavelength of the nanosecond laser is 500-1100 nm.

3. The cell edge isolation method according to claim 2, characterized in that: In step b, the laser pulse energy density is >0.3 J / cm 2 , the spot overlap rate is 5% to 90%, and the pulse width is 1 to 500ns.

4. The method for isolating the edge of a sliced ​​battery according to claim 1, characterized in that: In the step S30, after the isolation area is acid-washed and alkali-washed, the surface structure of the isolation area is a suede or flat structure.

5. The method for isolating the edge of a sliced ​​battery according to claim 4, characterized in that: In the step c, a hydrofluoric acid solution is used to perform pickling to remove the borosilicate glass, and an alkali solution is used to perform alkali washing to remove the boron emitter.

6. The cell edge isolation method according to claim 1, characterized in that: In the step b, the width of the isolation region formed by nanosecond laser opening is greater than 10 μm.

7. The cell edge isolation method according to claim 6, characterized in that: In the step f, the distance between the cutting part and the isolation area is less than 10 mm.

8. The method for isolating the edge of a sliced ​​battery according to any one of claims 1 to 7, characterized in that: Also includes the steps: g. Use alkali solution to etch the cutting area to remove the damaged layer; h. Prepare a side passivation layer on the cutting area.

9. The method for isolating the edge of a sliced ​​battery according to claim 8, characterized in that: In the step h, the side passivation layer prepared is AlO x With SiN x Laminated film.

10. A sliced ​​battery, characterized in that: The battery is prepared by the cell edge isolation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Semiconductor device with PN junction and preparation method thereof

    CN120112012A

  • Solar cell and preparation method thereof

    CN120187111A

  • Solar cell and preparation method thereof

    CN120187111B

  • Preparation method of battery piece, battery piece and photovoltaic module

    CN120897561A

  • A method for manufacturing a battery piece, a battery piece and a photovoltaic module

    CN120897561B