Broadband efficient microwave electromagnetic shielding composite film and preparation method thereof
Through Cu-Fe20Ni80-Cu/Ni composite multi-layer film structure and laser etching technology, conductive magnetic composite films were prepared, solving the problems of existing electromagnetic shielding materials in miniaturization, high integration, wide frequency and high efficiency, and achieving 0.1- The high-efficiency electromagnetic shielding of 80 to 100dB in the 40GHz frequency band fills the gap in the wide-band high-efficiency electromagnetic shielding film material.
Patent Information
- Application Number
- CN202411143010.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
The existing electromagnetic shielding materials have defects in lightweight, thin film, multi-functional integration, extreme environment resistance and low-cost and reliable manufacturing, and are difficult to meet the functional performance requirements of miniaturization, high integration, wideband and high efficiency.
Using Cu-Fe20Ni80-Cu/Ni (periodic structural unit) composite multi-layer film structure, metal Cu film, Ni80Fe20 alloy film and diamond-shaped periodic structural unit are prepared by magnetron sputtering coating and laser etching technology to form a conductive and magnetic composite film , realize the wide frequency efficiency of electromagnetic shielded composite film.
Achieving an electromagnetic shielding effect of 80 to 100dB in the frequency band of 0.1-40GHz, breaking through the skin depth limitation of a single type of conductive material, significantly improving the shielding effect of the wide band, and reducing the material thickness.
Smart Images

Figure CN119031685A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electromagnetic shielding, and in particular relates to a broadband and high-efficiency microwave electromagnetic shielding composite film and a preparation method thereof. Background Art
[0002] At present, the electromagnetic shielding materials that have been widely used in electronic equipment products are mainly metal plates. Traditional electromagnetic shielding composite materials represented by high-conductive metal particles filled with polymer resins and high-conductive metal material structural parts, when the thickness reaches the mm level or above, the shielding of electromagnetic field radiation can easily obtain a shielding effectiveness of more than 80dB-100dB. For example, the shielding effectiveness of 2mm pure copper plates can meet the requirements. However, the defects in lightweight, thin film, multi-functional integration, resistance to extreme service environment, low-cost and reliable manufacturing are becoming increasingly prominent, and it is difficult to meet new requirements such as miniaturization, high integration, broadband and high efficiency and other functional / performance attributes. Summary of the invention
[0003] In view of the technical problems that the above-mentioned shielding materials are difficult to meet the functional / performance attributes of miniaturization, high integration, broadband and high efficiency, the present invention provides a broadband and high-efficiency microwave electromagnetic shielding composite film and a preparation method thereof, which solves the problem of broadband and high efficiency of thin film materials for highly integrated communication equipment and achieves an electromagnetic shielding efficiency of 80 to 100 dB in the 0.1-40 GHz frequency band.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0005] A broadband and high-efficiency microwave electromagnetic shielding composite film, comprising a metal Cu film, a Ni 80 Fe 20 Alloy film, rhombus periodic structure unit and PCB board, the surface of the PCB board is grown with a metal Cu film, the surface of the metal Cu film is grown with Ni 80 Fe 20 Alloy thin film, the Ni 80 Fe 20 Rhombus-shaped periodic structural units grow on the surface of the alloy film.
[0006] The material of the rhombus periodic structural unit is metal Cu or metal Ni.
[0007] The thickness of the metal Cu film is in the range of 15 μm-19 μm, and the Ni 80 Fe 20 The thickness of the alloy film ranges from 100nm to 300nm.
[0008] The thickness of the diamond periodic structure unit using metal Cu is in the range of 5 μm-9 μm, and the thickness of the diamond periodic structure unit using metal Ni is in the range of 8 μm-12 μm.
[0009] A method for preparing a broadband and high-efficiency microwave electromagnetic shielding composite film comprises the following steps:
[0010] S1. Preparing a metal Cu film on the surface of a PCB board by a magnetron sputtering vacuum coating device;
[0011] S2. Preparation of Ni on the surface of metal Cu film 80 Fe 20 alloy film;
[0012] S3, in Ni 80 Fe 20 Metal Cu rhombus periodic structural units or metal Ni rhombus periodic structural units are prepared on the surface of the alloy film.
[0013] The method for preparing the metal Cu film in S1 is: using a multi-target magnetron sputtering coating equipment, using copper with a purity of 99.9% as the sputtering target, Ar as the sputtering process gas, and depositing the metal Cu film on the surface of the PCB board. The process conditions are a temperature of 180°C-220°C, a sputtering power of 250W, and an Ar flow rate of 50SCCM-55SCCM.
[0014] The S2 is used to prepare Ni 80 Fe 20 The method of alloy film is: using multi-target magnetron sputtering coating equipment, with Ni with a purity of 99.9% 80 Fe 20 Alloy is the sputtering target, Ar is the sputtering process gas, and Ni is deposited on the surface of the PCB board based on the metal Cu film. 80 Fe 20 Alloy film, the process conditions are temperature of 180-220℃, sputtering power of 1500W, and Ar flow rate of 50SCCM-55SCCM.
[0015] The method for preparing the metal Cu diamond periodic structure unit in S3 is: using a multi-target magnetron sputtering coating device, using metal Cu with a purity of 99.9% as a sputtering target material and Ar as a sputtering process gas, depositing a metal Cu film, Ni 80 Fe 20 A metal Cu film is continuously deposited on the basis of the alloy film, with a process temperature of 180°C-220°C, a sputtering power of 250W, an Ar flow rate of 50SCCM-55SCCM, and a FSS pattern is prepared on the metal Cu film.
[0016] The method for preparing the metal Ni rhombus periodic structure unit in S3 is: using a multi-target magnetron sputtering coating device, using Ni with a purity of 99.9% as a sputtering target material and Ar as a sputtering process gas, to deposit a metal Cu film, Ni 80 Fe 20 A metal Ni film is continuously deposited on the basis of the alloy film, with a process temperature of 240°C-280°C, a sputtering power of 450W, an Ar flow rate of 50SCCM-55SCCM, and a FSS pattern is prepared on the metal Ni film.
[0017] The method for preparing the diamond periodic structure unit (FSS) pattern: using laser etching equipment, the laser source wavelength is 1064nm, the processing parameters are: processing laser frequency: 200kHz, current 30%, focal length: 8.65mm, processing rate: 2mm / s.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention adopts Cu-Fe 20 Ni 80 -Cu / Ni (periodic structural unit) composite multilayer film structure design, the conductive and magnetic composite film material is organically combined with the frequency selective surface (FSS) to form a composite guided conductive film material. According to the electromagnetic shielding principle, the metal shielding film shields the far-field of the radiation interference source by reflecting and absorbing electromagnetic waves, that is, it simultaneously shields the electric field and magnetic field components generated by the field source. When a single type of conductive material is used, as the frequency increases, when the skin depth of the material is reached, the shielding effectiveness against the interference source will not increase with the increase of the material thickness; in order to significantly improve the high shielding effectiveness in the wide frequency band, a variety of composite conductive and magnetic film materials are used, and through reasonable impedance matching and resonant absorption design, the limitation of the skin depth of a single type of conductive material is broken. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0021] The structures, proportions, sizes, etc. illustrated in this specification are only used to match the contents disclosed in the specification so as to facilitate understanding and reading by persons familiar with the technology. They are not used to limit the conditions under which the present invention can be implemented, and therefore have no substantial technical significance. Any structural modification, change in proportion or adjustment of size shall still fall within the scope of the technical contents disclosed in the present invention without affecting the effects and purposes that can be achieved by the present invention.
[0022] Figure 1 It is a structural schematic diagram of the present invention;
[0023] Figure 2 This is a schematic diagram of a diamond-shaped periodic structural unit pattern of the present invention;
[0024] Figure 3 It is a shielding effectiveness test curve diagram of the broadband and high-efficiency microwave electromagnetic shielding composite film of the present invention.
[0025] Among them: 1 is metal Cu film, 2 is Ni 80 Fe 20 Alloy film, 3 is a diamond periodic structure unit, and 4 is a PCB board. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. These descriptions are only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0027] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0028] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0029] like Figure 1 As shown, the broadband high-efficiency microwave electromagnetic shielding composite film material is composed of metal Cu film 1, Fe20 Ni 80 The composite film material is composed of an alloy film 2 and a rhombus periodic structure unit 3, and is attached to the surface of a PCB board 4 substrate.
[0030] The metal Cu film 1, Ni 80 Fe 20 Alloy film 2, metal Cu film or Ni film of different types and thicknesses of metal or metal alloy film materials, wherein the diamond periodic structure unit 3 of the metal Cu film or Ni film is prepared by laser etching equipment to prepare a diamond periodic structure, and finally a broadband and high-efficiency electromagnetic shielding composite film material is prepared.
[0031] The thickness of the metal Cu film 1 ranges from 15 to 19 μm, and the optimal thickness is 17 μm. Preparation method: using multi-target magnetron sputtering coating equipment, using copper with a purity of 99.9% as the sputtering target, Ar as the sputtering process gas, the metal Cu film 1 is deposited on the surface of the PCB board, the process conditions are a temperature of 180-220°C, a sputtering power of 250W (set value), an Ar flow rate of 50-55SCCM, and the thickness of the deposited film is controlled by the substrate movement rate and the number of movements according to actual conditions.
[0032] Ni 80 Fe 20 The thickness of the alloy film 2 ranges from 100 nm to 300 nm, with an optimal thickness of 200 nm;
[0033] Ni 80 Fe 20 Alloy film 2 preparation method: using multi-target magnetron sputtering coating equipment, with a purity of 99.9% Ni 80 Fe 20 Alloy is the sputtering target, Ar is the sputtering process gas, and Ni is deposited on the basis of Cu film deposited on the surface of PCB board. 80 Fe 20 Alloy film 2, the process conditions are temperature of 180-220°C, sputtering power of 1500W (set value), Ar flow rate of 50-55SCCM, and the thickness of the deposited film is controlled by the substrate movement rate and the number of movements according to the actual conditions.
[0034] The thickness of the diamond periodic structure unit 3 of metal Cu ranges from 5 μm to 9 μm, with an optimal thickness of 7 μm; the FSS pattern size is: diamond, such as Figure 2 As shown; Cu film preparation method: using multi-target magnetron sputtering coating equipment, with 99.9% purity Cu as sputtering target material, Ar as sputtering process gas, depositing metal Cu film 1, Ni on the surface of PCB board 80 Fe 20The metal Cu film is deposited on the alloy film 2, the process temperature is 180-220°C, the sputtering power is 250W (set value), the Ar flow rate is 50-55SCCM, and the thickness of the deposited film is controlled by the substrate movement rate and movement times according to actual conditions. Method for preparing the Cu film diamond periodic structure unit (FSS) pattern: using laser etching equipment (laser source wavelength 1064nm), processing parameters: processing laser frequency: 200kHz, current 30%, focal length: 8.65mm, processing rate: 2mm / s.
[0035] The thickness of the diamond periodic structure unit 3 of metal Ni ranges from 8 μm to 12 μm, with the optimal thickness being 10 μm; the FSS pattern size is: diamond (see Figure 2 ); Ni film preparation method: using multi-target magnetron sputtering coating equipment, with Ni with a purity of 99.9% as the sputtering target and Ar as the sputtering process gas, a metal Cu film 1, Ni is deposited on the surface of the PCB board 80 Fe 20 A metal Ni film is deposited on the basis of alloy film 2, the process temperature is 240-280°C, the sputtering power is 450W (set value), the Ar flow rate is 50-55SCCM, and the thickness of the deposited film is controlled by the substrate movement rate and the number of movements according to actual conditions. Preparation method of Ni film diamond periodic structure unit (FSS) pattern: using laser etching equipment (laser source wavelength 1064nm), processing parameters: processing laser frequency: 200kHz, current 30%, focal length: 8.65mm, processing rate: 2mm / s.
[0036] The shielding effectiveness of broadband high-efficiency electromagnetic shielding composite film materials is tested according to GB / T12190-2006 standard, with the test sample ≥300mm×300mm, and the test results meet the requirements of reaching 80-100dB or above in the frequency band of 0.1~40GHz. This broadband high-efficiency electromagnetic shielding film material not only solves the problem of broadband high-efficiency shielding effectiveness, but also effectively reduces the thickness of the material and other issues, fundamentally filling the gap of broadband high-efficiency electromagnetic shielding film materials.
[0037] Shielding effectiveness of existing metal shielding materials
[0038] The shielding materials used in shielded rooms built in the United States have been tested and the shielding effectiveness of pure copper with a thickness of 100 μm is between 48 dB and 82 dB in the frequency range of 0.1 to 40 GHz (see Table 1).
[0039] Table 1 Shielding effectiveness of pure copper with a thickness of 100 μm used in shielded rooms built in the United States
[0040] Frequency / Hz 0.1G 0.45G 1G 5G 10G 18G 26.5G 40G Shielding effectiveness / dB 55 48 79 80 76 65 82 80
[0041] The technical indicators achieved by the present invention are:
[0042] The shielding effectiveness of the novel broadband high-efficiency electromagnetic shielding film designed by the present invention is as follows: the shielding effectiveness of the composite film material with a thickness of 24.2 μm is 81 dB to 99 dB in the frequency range of 0.1 to 40 GHz (see Table 2), the shielding effectiveness of the composite film material with a thickness of 27.2 μm is 81 dB to 96 dB in the frequency range of 0.1 to 40 GHz (see Table 3), and the shielding effectiveness of the composite film material with a thickness of 34.2 μm is 81 dB to 119 dB in the frequency range of 0.1 to 40 GHz (see Table 4). The shielding effectiveness test diagrams of Tables 1 to 4 are shown in Table 4. Figure 3 .
[0043] Table 2 Shielding effectiveness of the novel broadband high-efficiency electromagnetic shielding film with a thickness of 24.2 μm of the present invention
[0044]
[0045] Table 3 Shielding effectiveness of the novel broadband high-efficiency electromagnetic shielding film with a thickness of 27.2 μm of the present invention
[0046] Frequency / Hz 0.1G 0.45G 1G 5G 10G 18G 26.5G 40G Shielding effectiveness / dB 96 86 83 84 82 81 89 88
[0047] Table 4 Shielding effectiveness of the novel broadband high-efficiency electromagnetic shielding film with a thickness of 34.2 μm of the present invention
[0048] Frequency / Hz 0.1G 0.45G 1G 5G 10G 18G 26.5G 40G Shielding effectiveness / dB 119 110 99 84 81 82 96 91
[0049] Example 1: Cu film-Ni is used on one side of the PCB board 4 80 Fe 20 Alloy film-Cu film.
[0050] 1) Broadband high-efficiency microwave electromagnetic shielding composite film uses a 2mm thick PCB board as the substrate, and a 17μm thick Cu film, a 200nm thick Ni film and a 80 Fe 20 Alloy film-Cu film with a thickness of 7μm;
[0051] 2) The metal Cu film and Ni 80 Fe 20 The alloy film was coated by a multi-target magnetron sputtering device, and the diamond periodic structure unit of the outer Cu film was etched by a laser (laser source wavelength 1064nm).
[0052] Example 2: Cu film-Ni is used on one side of the PCB board 80 Fe 20 Alloy film-Ni film.
[0053] 1) Broadband high-efficiency microwave electromagnetic shielding composite film uses a 2mm thick PCB board as the substrate, and a 17μm thick Cu film, a 200nm thick Ni film and a 80 Fe 20 Alloy film-Ni film with a thickness of 10μm;
[0054] 2) Among them, metal Cu film, Ni 80 Fe 20 The alloy film and the Ni film were coated by multi-target magnetron sputtering equipment, and the diamond periodic structure unit of the outer Ni film was etched by laser equipment (laser source wavelength 1064nm).
[0055] Example 3: Cu film-Ni is used on one side of the PCB board 80 Fe 20 Alloy thin films - Cu thin films and Ni thin films.
[0056] 1) Broadband high-efficiency microwave electromagnetic shielding composite film uses a 2mm thick PCB board as the substrate, and a 17μm thick Cu film, a 200nm thick Ni film and a 80 Fe 20 Alloy film - 7μm thick Cu film and 10μm thick Ni film;
[0057] 2) Among them, metal Cu film, Ni 80 Fe 20 The alloy film and the Ni film were coated by multi-target magnetron sputtering equipment, and the diamond periodic structure units of the outer Cu film and the Ni film were etched by laser equipment (laser source wavelength 1064nm).
[0058] Only the preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention, and various changes should be included in the protection scope of the present invention.
Claims
1. A broadband and high-efficiency microwave electromagnetic shielding composite film, characterized in that: Including metal Cu film (1), Ni 80 Fe 20 Alloy film (2), rhombus periodic structure unit (3) and PCB board (4), wherein a metal Cu film (1) is grown on the surface of the PCB board (4), and Ni 80 Fe 20 Alloy film (2), the Ni 80 Fe 20 Rhombus-shaped periodic structural units (3) grow on the surface of the alloy film (2).
2. A broadband and high-efficiency microwave electromagnetic shielding composite film according to claim 1, characterized in that: The material of the rhombus periodic structural unit (3) is metal Cu or metal Ni.
3. The broadband and high-efficiency microwave electromagnetic shielding composite film according to claim 1, characterized in that: The thickness of the metal Cu film (1) is in the range of 15 μm to 19 μm, and the Ni 80 Fe 20 The thickness of the alloy film (2) is in the range of 100nm-300nm.
4. The broadband and high-efficiency microwave electromagnetic shielding composite film according to claim 2, characterized in that: The thickness of the metal Cu used in the diamond periodic structure unit (3) is in the range of 5 μm to 9 μm, and the thickness of the metal Ni used in the diamond periodic structure unit (3) is in the range of 8 μm to 12 μm.
5. A method for preparing a broadband and efficient microwave electromagnetic shielding composite film, characterized in that: The following steps are involved: S1. Preparing a metal Cu film on the surface of a PCB board by a magnetron sputtering vacuum coating device; S2. Preparation of Ni on the surface of metal Cu film 80 Fe 20 alloy film; S3, in Ni 80 Fe 20 Metal Cu rhombus periodic structural units or metal Ni rhombus periodic structural units are prepared on the surface of the alloy film.
6. The method for preparing a broadband high-efficiency microwave electromagnetic shielding composite film according to claim 5, characterized in that: The method for preparing the metal Cu film in S1 is: using a multi-target magnetron sputtering coating equipment, using copper with a purity of 99.9% as the sputtering target, Ar as the sputtering process gas, and depositing the metal Cu film on the surface of the PCB board. The process conditions are a temperature of 180°C-220°C, a sputtering power of 250W, and an Ar flow rate of 50SCCM-55SCCM.
7. The method for preparing a broadband high-efficiency microwave electromagnetic shielding composite film according to claim 5, characterized in that: The S2 is used to prepare Ni 80 Fe 20 The method of alloy film is: using multi-target magnetron sputtering coating equipment, with Ni with a purity of 99.9% 80 Fe 20 Alloy is the sputtering target, Ar is the sputtering process gas, and Ni is deposited on the surface of the PCB board based on the metal Cu film. 80 Fe 20 Alloy film, the process conditions are temperature of 180-220℃, sputtering power of 1500W, and Ar flow rate of 50SCCM-55SCCM.
8. The method for preparing a broadband high-efficiency microwave electromagnetic shielding composite film according to claim 5, characterized in that: The method for preparing the metal Cu diamond periodic structure unit in S3 is: using a multi-target magnetron sputtering coating device, using metal Cu with a purity of 99.9% as a sputtering target material and Ar as a sputtering process gas, depositing a metal Cu film, Ni 80 Fe 20 A metal Cu film is continuously deposited on the basis of the alloy film, with a process temperature of 180°C-220°C, a sputtering power of 250W, an Ar flow rate of 50SCCM-55SCCM, and a FSS pattern is prepared on the metal Cu film.
9. The method for preparing a broadband high-efficiency microwave electromagnetic shielding composite film according to claim 5, characterized in that: The method for preparing the metal Ni rhombus periodic structure unit in S3 is: using a multi-target magnetron sputtering coating device, using Ni with a purity of 99.9% as a sputtering target material and Ar as a sputtering process gas, to deposit a metal Cu film, Ni 80 Fe 20 A metal Ni film is continuously deposited on the basis of the alloy film, with a process temperature of 240°C-280°C, a sputtering power of 450W, an Ar flow rate of 50SCCM-55SCCM, and a FSS pattern is prepared on the metal Ni film.
10. The method for preparing a broadband high-efficiency microwave electromagnetic shielding composite film according to claim 8 or 9, characterized in that: The method for preparing the diamond periodic structure unit (FSS) pattern: using laser etching equipment, the laser source wavelength is 1064nm, the processing parameters are: processing laser frequency: 200kHz, current 30%, focal length: 8.65mm, processing rate: 2mm / s.