Transparent electrode and organic electroluminescent device
By using a composite layer of low-work function metal and high-work function metal in transparent electrodes, combining the optical coupling layer and passivation layer, the damage problem of transparent electrode materials during high temperature treatment in the prior art is solved, and high transmittance is achieved and low resistance electrodes ensure balanced luminescence and durability on both sides of the organic electroluminescent device.
Patent Information
- Application Number
- CN202410973979.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-26
AI Technical Summary
Existing transparent electrode materials are prone to damage organic electroluminescent/photovoltaic devices during high temperature treatment, and it is difficult to balance conductivity and light transmittance, resulting in a degradation of device performance.
Using a composite layer of low-work function metal and high-work function metal, combined with an optical coupling layer and a passivation layer, a transparent electrode is prepared by vacuum thermal evaporation method, a combination of low-work function metal such as Yb and high-work function metal such as Ag, and an optical coupling layer Materials such as BCP, passivation layer materials such as NaF, optimize the thickness and refractive index of the electrode to improve transmittance and conductivity.
It realizes transparent electrodes with high transmittance, low resistance and long life, ensuring balanced luminescence on both sides of the device, resistant to water vapor and oxygen, and improving the performance and service life of organic electroluminescent devices.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrode materials, and in particular to a transparent electrode and an organic electroluminescent device. Background Art
[0002] With the continuous development of display lighting and photovoltaic fields, people have put forward higher requirements for the efficiency of photovoltaic devices and have also developed a yearning for transparent devices. As a photoelectric device, a transparent or semi-transparent electrode is required to realize light output or light input on at least one side. The higher the transmittance of the electrode, the more light can pass through, and the device performance is often better. At present, the materials of transparent electrodes can be divided into: composite metal electrodes (such as Mg:Ag, Yb:Ag), dielectric / metal / dielectric (DMD) electrodes (such as MoO3 / Ag / MoO3, WO3 / Ag / WO3), transparent conductive oxide electrodes (such as ITO, AZO), nanomaterial electrodes (such as silver nanowires AgNW, CuNW, carbon nanotubes), graphene electrodes, etc. The difference in electrode materials determines the difference in their preparation methods. For example, metal nanowire electrodes are usually prepared by solution method, while ITO electrodes are prepared by sputtering deposition method and annealing is required to ensure good transmittance.
[0003] For organic electroluminescent / photovoltaic devices prepared by vacuum thermal evaporation, since the organic materials deposited are often not resistant to high temperatures and the density is not high enough, high-energy and high-temperature methods such as magnetron sputtering and chemical vapor deposition are easy to damage the organic materials, resulting in a decrease in device performance. At the same time, since the organic materials deposited in vacuum are often sensitive to water and oxygen, the electrodes prepared by the solution method will also damage the device. At present, the best method is to prepare the electrodes by vacuum thermal evaporation, which can avoid water and oxygen while also facilitating preparation. In order to ensure good conductivity of the electrode, high-work function metals with good conductivity (such as Ag, Au, Al) are often required to participate, but a single high-work function metal also has the problem of poor electron injection ability. In order to improve the transmittance of the electrode, the most direct and effective method is to reduce its thickness, but the reduction in thickness will lead to an increase in resistivity, and it is difficult to balance conductivity and transmittance. Summary of the invention
[0004] In order to overcome at least one technical problem existing in the above-mentioned prior art, one of the objectives of the present invention is to provide a transparent electrode.
[0005] A second object of the present invention is to provide a device.
[0006] A third object of the present invention is to provide an application of a transparent electrode in electronic products.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] The first aspect of the present invention provides a transparent electrode, comprising a composite metal layer, a light coupling layer, and a passivation layer stacked in sequence; the composite metal layer comprises a low work function metal and a high work function metal; the low work function metal is selected from at least one of Yb, Ca, Rb, Cs, Y, Li, Na, and K; the high work function metal is selected from at least one of Ag, Au, Al, Cu, Mo, Ni, and Sn.
[0009] Preferably, the material of the optical coupling layer is selected from at least one of bathocuproin, 4,7-diphenyl-1,10-phenanthroline, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, MoO3, and WO3. In the present invention, the optical coupling layer can improve the transmittance of light.
[0010] Preferably, the material of the passivation layer is selected from at least one of NaF, MgF2, LiF, MoO3, WO3, ZnS, ZnSe, and SiO2; more preferably, the material of the passivation layer is NaF. In the present invention, the passivation layer plays a role in isolating water vapor and oxygen on the one hand, and can protect the electrode from damage during electrode processing on the other hand.
[0011] Preferably, the thickness of the passivation layer is 1 to 500 nm; further preferably, the thickness of the passivation layer is 1 to 50 nm; more preferably, the thickness of the passivation layer is 5 to 20 nm.
[0012] Preferably, the refractive index n2 of the passivation layer is 1.4-2, and the refractive index n2 of the passivation layer is ≤ the refractive index n1 of the optical coupling layer.
[0013] Preferably, the light transmittance of the passivation layer at a wavelength of 380 nm to 780 nm is not less than 90%.
[0014] Preferably, the low work function metal is Yb.
[0015] Preferably, the high work function metal is selected from Ag, Au or a combination thereof.
[0016] Preferably, the mass ratio of the low work function metal to the high work function metal is 1:(1-9). The high work function metal has good electrical conductivity, and the low work function metal has high light transmittance.
[0017] Preferably, the light transmittance of the low work function metal is ≥80% when the layer thickness is 5 nm and the wavelength is 420-780 nm.
[0018] Preferably, the thickness of the composite metal layer electrode is 5 to 20 nm; further preferably, the thickness of the composite metal layer electrode is 8 to 15 nm.
[0019] Preferably, the thickness of the optical coupling layer is 1 to 500 nm; further preferably, the thickness of the optical coupling layer is 5 to 200 nm.
[0020] Preferably, the refractive index n1 of the material of the optical coupling layer is 1.4-2.
[0021] Preferably, the light transmittance of the optical coupling layer at a wavelength of 380 nm to 780 nm is not less than 90%.
[0022] Preferably, the optical coupling layer is formed by vacuum evaporation deposition of at least one material selected from 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline (BCP), 4,7-diphenyl-1,10-phenanthroline (Bphen), N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPB), 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (TPD), MoO3, and WO3.
[0023] Preferably, the light transmittance of the transparent electrode at a wavelength of 420-780 nm is not less than 60%; further preferably, the light transmittance of the transparent electrode at a wavelength of 540-680 nm is not less than 80%.
[0024] Preferably, the resistance of the transparent electrode is ≤200Ω / □.
[0025] Preferably, the composite metal layer, the optical coupling layer and the passivation layer are all made by a continuous vacuum thermal evaporation coating method.
[0026] The transparent electrode in the present invention can be prepared by a vacuum thermal evaporation deposition method, and the preparation method is simple and easy to operate.
[0027] The second aspect of the present invention provides a device, comprising the transparent electrode provided in the first aspect of the present invention; the device includes an organic electroluminescent device and a photovoltaic device.
[0028] Preferably, the organic electroluminescent device comprises an anode, an organic light-emitting unit, and a cathode stacked in sequence; the cathode is the transparent electrode provided in the first aspect of the present invention; further preferably, the organic electroluminescent device comprises a substrate, an anode, an organic light-emitting unit, and a cathode stacked in sequence.
[0029] Preferably, the material of the substrate is selected from a glass substrate and a flexible film substrate. The substrate can be any transparent substrate material that can be used in OLED display, lighting, organic photovoltaic and other devices in the prior art. The substrate can also be an opaque substrate, in which case light can only be emitted from the cathode side. If the substrate is a transparent material, the cathode side and the substrate side can emit light at the same time.
[0030] Preferably, the organic light-emitting unit comprises a hole injection layer, a hole transport layer, an electron blocking layer, an organic light-emitting layer, a hole blocking layer, an electron transport layer, and an electron injection layer which are stacked in sequence.
[0031] Preferably, the organic light-emitting unit comprises a hole injection layer, a hole transport layer, an organic light-emitting layer, and an electron transport layer which are stacked in sequence.
[0032] The third aspect of the present invention provides application of the transparent electrode described in the first aspect of the present invention in electronic products.
[0033] The beneficial effects of the present invention are as follows: the transparent electrode of the present invention adopts a compound of low work function metal and high work function metal, which can ensure that the transparent electrode has good conductivity on the one hand, and can improve the electron injection ability and the film quality of the transparent electrode on the other hand, and the ohmic contact between the low work function metal and the electron transport material can promote electron injection. In addition, the transparent electrode of the present invention has high light transmittance, thin thickness and long service life.
[0034] The two sides of the organic electroluminescent device in the present invention have extremely high light transmittance, which can achieve symmetrical and balanced light emission on both sides of the device. The light emission effect is better than that of the single-sided light-emitting device in the prior art. In addition, the device in the present invention is resistant to water vapor and oxygen and has a long service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Schematic diagram of the structure of the organic electroluminescent device in Example 3.
[0036] Figure 2 It is a transmittance test diagram of the organic electroluminescent device in Comparative Examples 1 to 3.
[0037] Figure 3 It is a transmittance test diagram of the organic electroluminescent device in Comparative Example 3 and Example 1.
[0038] Figure 4 This is a transmittance test diagram of the organic electroluminescent device in Example 1 and Example 2.
[0039] Figure 5 This is a transmittance test diagram of the organic electroluminescent device in Examples 2 to 5.
[0040] Figure 6 This is a device life test diagram of the organic electroluminescent devices in Example 2 and Example 4. DETAILED DESCRIPTION
[0041] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.
[0042] The raw material information used in the examples and comparative examples of the present invention is as follows:
[0043] ITO: Indium Tin Oxide;
[0044] HAT-CN: 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene;
[0045] NPB: N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine;
[0046] Bepp2: bis(2-(2-phenolyl)pyridinium)beryllium;
[0047] Ir(ppy)3: tris(2-phenylpyridine)iridium;
[0048] Bphen: 4,7-diphenyl-1,10-phenanthroline;
[0049] Liq: 8-hydroxyquinoline lithium;
[0050] BCP: 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline
[0051] NaF: Sodium Fluoride
[0052] Example 1
[0053] This example provides an organic electroluminescent device, including a substrate, a transparent anode, an organic light-emitting unit, and a cathode stacked in sequence, wherein the cathode is a composite metal electrode. The structure of the organic light-emitting unit is a hole injection layer, a hole transport layer, a green light-emitting layer, and an electron transport layer stacked in sequence, the material of the transparent anode is ITO, and the organic light-emitting unit and the cathode are continuously obtained by vacuum thermal evaporation coating in a vacuum environment. The material of the hole injection layer of the device is HAT-CN, and the thermal evaporation rate is controlled to be 0.1nm / s, and a film with a thickness of 50nm is finally obtained; the material of the hole transport layer is NPB, and the thermal evaporation rate is controlled to be 0.1nm / s, and the thickness is 20nm; the thickness of the green light-emitting layer is 30nm, and the thermal evaporation rates are controlled to be 0.1nm / s and 0.005nm / s respectively, and the final green light-emitting layer is a film composed of Bepp2 and Ir(ppy)3 with a mass ratio of 95:5. The thickness of the electron transport layer is 30nm, and the thermal evaporation rates are controlled to be 0.1nm / s and 0.07nm / s, respectively, and Bphen and Liq are co-evaporated to obtain a film with a mass ratio of 100:70 for the electron transport layer. For the composite metal electrode, the thermal evaporation rates are controlled to be 0.1nm / s and 0.1nm / s, respectively, to obtain a film composed of Yb and Ag with a mass ratio of 1:1, and a thickness of 12nm. The material of the optical coupling layer is BCP, and the thermal evaporation rate is 0.1nm / s to obtain a film with a thickness of 50nm. The device structure in this example is: ITO / HAT-CN (50nm) / NPB (20nm) / Bepp2:Ir(ppy)3 (30nm, 5%) / Bphen:Liq (30nm, 70%) / Yb:Ag (1:1, 12nm).
[0054] Example 2
[0055] This example provides an organic electroluminescent device, including a substrate, a transparent anode, a hole injection layer, a hole transport layer, a green light-emitting layer, an electron transport layer and a cathode stacked in sequence. The structure of the cathode is a two-layer structure of a composite metal electrode and a light coupling layer stacked, and the composite metal electrode is located between the electron transport layer and the light coupling layer. The material of the transparent anode is ITO, the material of the hole injection layer is HAT-CN, and the thickness is 50nm; the material of the hole transport layer is NPB, and the thickness is 20nm; the thickness of the green light-emitting layer is 30nm, and the green light-emitting layer is composed of Bepp2 and Ir(ppy)3 with a mass ratio of 95:5. The thickness of the electron transport layer is 30nm, and the electron transport layer is made by co-evaporation doping of Bphen and Liq with a mass ratio of 100:70. The composite metal electrode is composed of Yb and Ag with a mass ratio of 1:1, and its thickness is 12nm. The material of the light coupling layer is BCP, and its thickness is 50nm. The organic electroluminescent device in this example is: ITO / HAT-CN (50nm) / NPB (20nm) / Bepp2:Ir(ppy)3 (30nm, 5%) / Bphen:Liq (30nm, 70%) / Yb:Ag (1:1, 12nm) / BCP (50nm).
[0056] Example 3
[0057] like Figure 1 As shown, the difference between the organic electroluminescent device in this example and Example 2 is that: a passivation layer is provided on the surface of the optical coupling layer in this example, the material of the passivation layer is NaF, the thermal evaporation rate is 0.05nm / s, and the thickness is 5nm. The device structure of the organic electroluminescent device in this example is: ITO / HAT-CN (50nm) / NPB (20nm) / Bepp2:Ir(ppy)3 (30nm, 5%) / Bphen:Liq (30nm, 70%) / Yb:Ag (1:1, 12nm) / BCP (50nm) / NaF (5nm).
[0058] Example 4
[0059] The organic electroluminescent device in this example is different from that in Example 3 in that the material of the passivation layer in this example is NaF, and the thickness is 10 nm. The device structure of the organic electroluminescent device in this example is: ITO / HAT-CN (50 nm) / NPB (20 nm) / Bepp2:Ir(ppy)3 (30 nm, 5%) / Bphen:Liq (30 nm, 70%) / Yb:Ag (1:1, 12 nm) / BCP (50 nm) / NaF (10 nm).
[0060] Example 5
[0061] The organic electroluminescent device in this example is different from that in Example 3 in that the material of the passivation layer in this example is NaF, and the thickness is 20 nm. The device structure of the organic electroluminescent device in this example is: ITO / HAT-CN (50 nm) / NPB (20 nm) / Bepp2:Ir(ppy)3 (30 nm, 5%) / Bphen:Liq (30 nm, 70%) / Yb:Ag (1:1, 12 nm) / BCP (50 nm) / NaF (20 nm).
[0062] Comparative Example 1
[0063] This example provides an organic electroluminescent device, including a substrate, a transparent anode, a hole injection layer, a hole transport layer, a green light-emitting layer, an electron transport layer and a semi-transparent cathode stacked in sequence. The material of the transparent anode is ITO, the material of the hole injection layer is HAT-CN, and the thickness is 50nm; the material of the hole transport layer is NPB, and the thickness is 20nm; the thickness of the green light-emitting layer is 30nm, and the green light-emitting layer is composed of Bepp2 and Ir(ppy)3 with a mass ratio of 95:5. The thickness of the electron transport layer is 30nm, and the electron transport layer is made by co-evaporation doping of Bphen and Liq with a mass ratio of 100:70. The semi-transparent cathode is composed of Mg and Ag with a mass ratio of 1:9, and its thickness is 20nm. The organic electroluminescent device in this example is ITO / HAT-CN (50 nm) / NPB (20 nm) / Bepp2:Ir(ppy)3 (30 nm, 5%) / Bphen:Liq (30 nm, 70%) / Mg:Ag (1:9, 20 nm).
[0064] Comparative Example 2
[0065] The organic electroluminescent device in this example is different from that in comparative example 1 only in that the thickness of the semi-transparent cathode in this example is 12 nm, and the device structure in this example is: ITO / HAT-CN (50 nm) / NPB (20 nm) / Bepp2:Ir(ppy)3 (30 nm, 5%) / Bphen:Liq (30 nm, 70%) / Mg:Ag (1:9, 12 nm).
[0066] Comparative Example 3
[0067] The organic electroluminescent device in this example is different from that in comparative example 2 only in that the mass ratio of Mg and Ag in the semi-transparent cathode in this example is 1:1, and the device structure in this example is: ITO / HAT-CN (50nm) / NPB (20nm) / Bepp2:Ir(ppy)3 (30nm, 5%) / Bphen:Liq (30nm, 70%) / Mg:Ag (1:1, 12nm).
[0068] Performance Test:
[0069] (1) Sheet resistance test
[0070] Mixed electrode layers with different layer thicknesses and different metal mass ratios were prepared on a transparent glass substrate by vacuum thermal evaporation coating method, specifically: A electrode layer: the mass ratio of Mg and Ag is 1:9, and the thickness is 20nm; B electrode layer: the mass ratio of Mg and Ag is 1:9, and the thickness is 12nm; C electrode layer: the mass ratio of Mg and Ag is 1:1, and the thickness is 12nm; D electrode layer: the mass ratio of Yb and Ag is 1:1, and the thickness is 12nm; then the A electrode layer, the B electrode layer, the C electrode layer and the D electrode layer are placed on a four-probe device under a N2 protection environment, and the square resistance of the A electrode layer, the B electrode layer, the C electrode layer and the D electrode layer is tested by the four-probe method. The specific test results are shown in Table 1 below:
[0071] Table 1 Sheet resistance test results
[0072] Test Group Electrode parameters Sheet resistance A electrode layer Mg:Ag (1:9, 20nm) 4Ω / □ B electrode layer Mg:Ag (1:9, 12nm) 7Ω / □ C electrode layer Mg:Ag (1:1, 12nm) 16Ω / □ D electrode layer Yb:Ag (1:1, 12nm) 14Ω / □
[0073] As shown in Table 1, in the Mg:Ag system, the resistance of the film increases with the increase of Mg content at the same thickness; at the same material ratio, the resistance decreases with the increase of thickness. At the same thickness, such as 12nm, the resistance of Yb:Ag (1:1) is slightly smaller than that of Mg:Ag. Therefore, the square resistance of the cathode can be adjusted by adjusting the thickness, material and material ratio of the cathode.
[0074] (2) Transmittance test
[0075] The transmittance of the organic electroluminescent devices in Comparative Examples 1 to 3 at wavelengths of 380 to 780 nm was tested respectively. The specific test results are as follows: Figure 2 As shown. Figure 2 It can be seen that the transmittance of the organic electroluminescent devices in Comparative Examples 1 to 3 at wavelengths of 380 to 780 nm is greater than 40%, among which the transmittance of the organic electroluminescent device in Comparative Example 2 is better, and the transmittance can reach 85.6%. When the raw materials for preparing the mixed electrode layer are the same, the transmittance decreases with the increase of the thickness of the mixed electrode layer. For example, the transmittance of the organic electroluminescent device in Comparative Example 1 is 52.9% at a wavelength of 620 nm, and it has a strong reflection; the thickness of the semi-transparent cathode in Comparative Example 2 is smaller than that of Comparative Example 1, and its transmittance is significantly improved, and the transmittance at a wavelength of 620 nm is increased to 75.9%. The mass ratio of Mg and Ag in Comparative Example 3 is 1:1, and the transmittance at a wavelength of 620 nm reaches 62.1%. When the thickness of the mixed electrode layer is the same, the mass ratio of Mg and Ag will affect the transmittance of the mixed electrode layer.
[0076] The transmittance of the organic electroluminescent devices in Example 1 and Comparative Example 3 at a wavelength of 380 to 780 nm was tested. The specific test results are as follows: Figure 3 As shown. Figure 3 It can be seen that the transmittance of the organic electroluminescent devices in Example 1 and Comparative Example 3 at 380-780 nm is greater than 60%. Due to the higher transmittance of Yb itself, Example 1 has a higher transmittance than Comparative Example 3. At a wavelength of 620 nm, the transmittance is increased from 62.1% to 76.4%.
[0077] The transmittance of the organic electroluminescent device in Examples 1 to 2 was tested at a wavelength of 380 to 780 nm. The specific test results are as follows: Figure 4 As shown. Figure 4 It can be seen that the transmittance of the device obtained by evaporating a light coupling layer BCP on the composite metal electrode in Example 1 is significantly improved, specifically: the transmittance at 460nm, 530nm, and 620nm reaches 84%, 85%, and 84.5%.
[0078] The transmittance of Examples 2 to 5 at wavelengths of 380 to 780 nm was tested respectively. The specific test results are as follows: Figure 5 As shown. Figure 5 It can be seen that setting a NaF passivation layer on the surface of the optical coupling layer and different thicknesses of the NaF passivation layer will not affect the light transmittance of the cathode. Since the optical coupling layer and the low work function metal Yb are sensitive to water and oxygen, another passivation layer is deposited on the optical coupling layer. It is required that the passivation layer has little effect on the transmittance and can better isolate water and oxygen. The refractive index is preferably between the optical coupling layer and the air. The above-mentioned NaF passivation layer can meet the requirements. Based on cost considerations, when the thickness of the NaF passivation layer is 10nm, both cost and passivation effect can be taken into account.
[0079] (3) Device performance test
[0080] The organic electroluminescent devices in Examples 1 to 2, Example 4 and Comparative Examples 1 to 3 are respectively connected to a power supply to make the green light-emitting layer emit light, and then the device performance is tested. The specific test method is: first, under a constant current I1, a spectroradiometer is used to test the brightness L1 and spectrum of the OLED device, and then the device is transferred to the test black box of the IVL system, and the constant current mode interface is used to select the corresponding RGB channel, and the current value I1 is set to be the same as the brightness of the OLED device tested by the spectroradiometer before, and the device is measured and then the silicon photodiode sensing brightness L2 in the black box is tested to obtain the corresponding test brightness ratio (also called correction factor) γ=L1 / L2, and then the constant current mode interface is switched to the test interface, and the test voltage range and the number of test points are set to start the test. The software automatically obtains the IVL curve, and the brightness corresponds to the brightness value sensed by the silicon photodiode. The brightness is multiplied by the correction factor γ to obtain the true brightness L of the QLED device, and finally the device IVL curve is drawn. The device current efficiency (LE) refers to the ratio of the outward luminous brightness of the device to the device current density, and the unit is candela per ampere (cd A -1 ); can be expressed by the following formula:
[0081]
[0082] Where L is the luminous brightness, unit is cd m -2 ; s is the effective light-emitting area of the device, unit: cm 2 ; J is the current density of the device when it is working, in mA cm -2 , Bottom (denoted as B) is the light emitted from the ITO side of the organic electroluminescent device, Top (denoted as T) is the light emitted from the cathode side of the organic electroluminescent device, and the light-on voltage (denoted as V on ) is the brightness of the device reaches 1cd / m 2 The working voltage at that time.
[0083] The performance of the organic electroluminescent devices in Example 2, Example 4 and Comparative Examples 1 to 3 measured according to the above test method is shown in Table 2 below. The performance of the organic electroluminescent device in Example 1 measured according to the above test method is shown in Table 3 below, where @1000 cd / m 2 Indicates brightness is 1000cd / m 2 Device performance, V represents the corresponding device voltage, J represents the corresponding current density, and LE represents the corresponding current efficiency of the device; @10mA / cm 2 It means that the device is under the condition of 10mA / cm 2 performance under , L is the corresponding device brightness.
[0084] Table 2 Performance test results of the organic electroluminescent devices in Example 2, Example 4 and Comparative Examples 1 to 3
[0085]
[0086] As shown in Table 2, in Comparative Example 1, the Mg:Ag electrode with a thickness of 20 nm and a mass ratio of 1:9 is used. The transmittance is not high enough and the reflection is strong. The L Top / L Bottom =0.316, that is, the intensity of the light emitted from the cathode side is only 1 / 3 of the intensity of the light emitted from the ITO side, indicating that the difference in the intensity of the light emitted from the cathode side and the ITO side of the device is large, which is not conducive to the application of transparent display devices. Comparative Example 2 reduces the thickness of the cathode to 12nm. Although the transmittance is significantly improved, the performance of the prepared device is poor, and the start-up voltage reaches 6V, which does not meet the device use requirements. Comparative Example 3 uses a Mg:Ag cathode with a mass ratio of 1:1, which has a better transmittance. At the same time, the prepared transparent device has better performance, and its L Top / L Bottom =0.568, that is, the intensity of the light emitted from the cathode side is more than 1 / 2 of the intensity of the light emitted from the ITO side. Compared with comparative examples 1 to 2, although the overall performance of comparative example 3 has been improved, the effect is still not good and cannot meet the use requirements of transparent display devices.
[0087] Table 3 Performance test results of the organic electroluminescent device in Example 1
[0088]
[0089] As shown in Table 3, in Example 1, Yb is used to replace Mg, and the transmittance of the electrode is significantly improved. The light intensity emitted from the cathode side of the device is L1 / 2 of the light intensity emitted from the ITO side. Top / L Bottom =0.802, showing good light-emitting performance on both sides. At the same time, the device lighting voltage and efficiency are better than those of comparative examples 1 to 3, and the device achieves a low voltage lighting, as low as 2.4V. Example 2 sets an optical coupling layer on the surface of the composite metal electrode, and the light intensity of the device from the cathode side is L1 / 2 of the light intensity from the ITO side. Top / L Bottom =0.934, the light output from both sides is further balanced, showing a better light output performance from both sides than that of Example 1. At the same time, the efficiency of the device is 45.8cd / A on both sides, which is a certain degree of improvement compared with Example 1. In Example 4, a passivation layer is added on the optical coupling layer, and the light intensity of the device from the cathode side is L1 / 2 of the light intensity from the ITO side. Top / L Bottom=0.954, the brightness of the light from both sides is balanced, showing excellent light output performance from both sides, which further confirms that the device has excellent transmittance.
[0090] (1) Device life test
[0091] The service life of the organic electroluminescent devices in Example 2 and Example 4 was tested respectively. The specific test method was as follows: a constant current was input into the life test instrument so that the initial brightness of the device was 10000 cd / m 2 , the system will record the brightness of the device at short intervals to draw a life curve of the device brightness over time. The results measured according to this test method are as follows Figure 6 As shown. Figure 6 It can be seen that the device life of Example 4 is significantly improved compared to the device life of Example 2 without the passivation layer. 2 Under this condition, the device brightness of Example 4 drops to 80% of the device life (T 80 ) is 307 hours, while under the same conditions, the device brightness of Example 2 drops to 80% of the device life (T 80 ) is 105 hours. Compared with Example 2, the device life of Example 4 is increased by nearly 3 times, further indicating that adding a passivation layer on the optical coupling layer can significantly increase the life of the organic electroluminescent device.
[0092] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A transparent electrode, characterized in that: It includes a composite metal layer, an optical coupling layer, and a passivation layer which are stacked in sequence; the composite metal layer includes a low work function metal and a high work function metal; the low work function metal is selected from at least one of Yb, Ca, Rb, Cs, Y, Li, Na, and K; the high work function metal is selected from at least one of Ag, Au, Al, Cu, Mo, Ni, and Sn.
2. The transparent electrode according to claim 1, characterized in that: The material of the optical coupling layer is selected from at least one of 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline, 4,7-diphenyl-1,10-phenanthroline, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, MoO3, and WO3; And / or, the optical coupling layer has a thickness of 1 to 500 nm; And / or, the light transmittance of the optical coupling layer at a wavelength of 380 nm to 780 nm is not less than 90%.
3. The transparent electrode according to claim 1, characterized in that: The material of the passivation layer is selected from at least one of NaF, MgF2, LiF, MoO3, WO3, ZnS, ZnSe, and SiO2; And / or, the thickness of the passivation layer is 1 to 500 nm; And / or, the light transmittance of the passivation layer at a wavelength of 380 nm to 780 nm is not less than 90%.
4. The transparent electrode according to claim 1, characterized in that: In the composite metal layer, the mass ratio of the low work function metal to the high work function metal is 1:(1-9); And / or, the thickness of the composite metal layer is 5 to 20 nm; And / or, the light transmittance of the low work function metal is ≥80% when the layer thickness is 5 nm and the wavelength is 420-780 nm.
5. The transparent electrode according to any one of claims 1 to 4, characterized in that: The light transmittance of the transparent electrode at a wavelength of 420nm to 780nm is not less than 60%; And / or, the resistance of the transparent electrode is ≤200Ω / □.
6. The transparent electrode according to any one of claims 1 to 4, characterized in that: The composite metal layer, the optical coupling layer and the passivation layer are all prepared by a continuous vacuum thermal evaporation coating method.
7. A device, characterized in that: It comprises the transparent electrode according to any one of claims 1 to 6; the device comprises an organic electroluminescent device and a photovoltaic device.
8. The device according to claim 7, characterized in that: The organic electroluminescent device comprises an anode, an organic light-emitting unit, and a cathode which are stacked in sequence; the cathode is the transparent electrode according to any one of claims 1 to 6.
9. The device according to claim 8, characterized in that: The organic light-emitting unit includes a hole injection layer, a hole transport layer, an organic light-emitting layer, and an electron transport layer which are stacked in sequence.
10. Use of the transparent electrode according to any one of claims 1 to 6 in electronic products.