Method for improving flexoelectric property of ferroelectric ceramic
By placing the ferroelectric ceramic in silicone oil and applying a DC voltage for polarization, the problem of limited improvement in the flexural electric effect of ferroelectric materials in the prior art is solved, and the significant improvement of the flexural electric coefficient and piezoelectric-flexural lining are achieved. Application expansion of electrical coupling.
Patent Information
- Application Number
- CN202411175759.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-26
AI Technical Summary
When the prior art improves the flexural electric effect response of ferroelectric materials, there are limitations on material stiffness and bending fracture strength, and the process complexity and material sensitivity brought about by the doping modification method are difficult to avoid damaging other properties. The flexural electric coefficient is significantly improved under the premise.
The ferroelectric ceramic after the electrode is coated is placed in silicone oil, and a DC voltage is applied for polarization, which significantly increases the flexural electrical coefficient of the ferroelectric ceramic.
A method to significantly improve the flexural electrical coefficient of ferroelectric ceramics is achieved, with strong operability and simple process, suitable for a variety of ferroelectric materials, meeting the requirements of piezoelectric-flexural electrical coupling of some devices, and the flexural electrical effect is increased by nearly 40. Time.
Smart Images

Figure CN119031814A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electromechanical coupling of functional materials, and in particular to a method for improving the flexoelectric performance of ferroelectric ceramics. Background Art
[0002] The flexoelectric effect is an electromechanical coupling phenomenon. When a material undergoes non-uniform deformation, it causes the separation of positive and negative charge centers, resulting in electrical polarization at the macroscopic level. This phenomenon is called the positive flexoelectric effect. Conversely, non-uniform polarization in space can also induce mechanical deformation of the material, which is called the inverse flexoelectric effect. These effects show broad application potential in the field of cutting-edge functional materials, especially in applications such as sensors, brakes, and energy storage. The magnitude of the flexoelectric effect is usually measured by the flexoelectric coefficient μ. ijkl To quantify, this coefficient shows significant differences in different materials. The flexoelectric coefficient of most dielectric materials is in the range of 0.1-1 nC / m, while the flexoelectric coefficient of ferroelectric materials is significantly higher than this value, usually 3 to 6 orders of magnitude larger than the theoretically calculated value. Previous studies have explained the abnormally high values of the flexoelectric coefficient in ferroelectric materials through mechanisms such as the preferential orientation of polar nanodomains and spontaneously polarized surface layers. Although the flexoelectric effect is more significant in ferroelectric materials, it is not prominent compared to the piezoelectric effect in many cases. Therefore, improving the flexoelectric response of materials is an ongoing and critical research goal.
[0003] In order to enhance the flexoelectric effect, researchers have tried a variety of methods. One method is to enhance the flexoelectric response by generating a larger strain gradient in the material through structural design, such as nanoarrays with truncated pyramid tips, films with wrinkled deformation, or using epitaxial strain to change the strain gradient of the film. However, these methods are limited by the stiffness and bending fracture strength of the material, and their enhancement effect is limited. Another method is to directly increase the flexoelectric coefficient of the material, which can be achieved by doping modification to enhance interface polarization, using graphite for asymmetric reduction to control the composition gradient, or by forming a spontaneously polarized surface layer by heat treatment above the Curie temperature. Although these methods can significantly improve the flexoelectric coefficient of the material, they also bring new problems, such as the sensitivity of the material to doping elements, the complexity of process control, and the limitations of the material in piezoelectric-flexoelectric coupling applications after semiconductorization. Therefore, a method is needed to effectively improve the flexoelectric coefficient of the material without compromising other properties of the material to solve the problems existing in the existing technology and expand its potential in piezoelectric-flexoelectric coupling applications. Summary of the invention
[0004] In view of the technical problems existing in the above-mentioned prior art, the present invention proposes a method for improving the flexoelectric performance of ferroelectric ceramics. The ferroelectric ceramics coated with electrodes are placed in silicone oil and a certain DC voltage is applied. After the pressurized treatment, the flexoelectric coefficient of the ferroelectric ceramics is significantly improved. This method of significantly improving the flexoelectric effect is applicable to a variety of ferroelectric materials.
[0005] The present invention provides a method for improving the flexoelectric properties of ferroelectric ceramics, the method comprising the following steps: Step 1, preparing ceramic powder; Step 2, preparing the synthesized ceramic powder into ferroelectric ceramics; Step 3, preparing metal electrodes on both surfaces of the ferroelectric ceramic; Step 4: placing the electrode-coated ferroelectric ceramic in silicone oil, applying a certain DC voltage, and performing polarization treatment to increase the flexoelectric coefficient of the ferroelectric ceramic.
[0006] The present invention has the following beneficial technical effects: (1) A method for significantly improving the flexoelectric coefficient of ferroelectric ceramics is proposed. This method does not require the design and processing of complex structures to improve the flexural properties. It is highly operable and has a simple process. (2) The present invention is applicable to most ferroelectric materials and has high universality; (3) The ferroelectric ceramics in the present invention are polarized to form a coupling of the interaction between the polarization electric field and the flexural electric field, which meets the requirements of some devices for the simultaneous use of piezoelectric effect and flexoelectric effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 Lead zirconate titanate (PbTi x Zr 1-x Schematic diagram of the flexoelectric coefficient of O3: PZT-based ferroelectric ceramics before and after polarization and after depolarization. DETAILED DESCRIPTION
[0008] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other. To achieve the above-mentioned purpose, the present invention adopts the following technical scheme.
[0009] The present invention provides a method for improving the flexoelectric properties of ferroelectric ceramics, the method comprising the following steps: Step 1, preparing ceramic powder; Step 2, preparing the synthesized ceramic powder into ferroelectric ceramics; Step 3, preparing metal electrodes on both surfaces of the ferroelectric ceramic; Step 4: placing the electrode-coated ferroelectric ceramic in silicone oil, applying a certain DC voltage, and performing polarization treatment to increase the flexoelectric coefficient of the ferroelectric ceramic.
[0010] Specifically, in step 1, the ceramic powder is prepared by solid phase reaction method; according to the chemical formula of the synthetic sample, the required content of each chemical raw material is calculated, and the raw materials that are easy to absorb water need to be dried before use. After weighing the materials according to the calculated results, anhydrous ethanol is added for ball milling for 6-12 hours, and then the slurry is dried and calcined in a muffle furnace to complete the synthesis of the ceramic powder.
[0011] In step 2, the synthesized ceramic powder is prepared into the required ferroelectric ceramics by using processes such as compression molding and tape casting. The specific operation of compression molding is as follows: the ceramic powder prepared in step 1 is granulated using a polyvinyl alcohol solution with a mass fraction of 5% to ensure that the powder has a certain fluidity. Then a certain mass of granulated powder is weighed and placed in a mold, and the powder is pressed and molded using a tablet press. Tape casting is to add a suitable solvent to the synthesized ceramic powder and then perform wet ball milling to obtain a stable and fluid slurry, and then use a scraper and other equipment to form ceramic embryo membranes of different thicknesses, and cut them as needed after drying. Since both methods introduce organic matter to assist molding during the molding process, other substances in them need to be removed by high-temperature treatment before sintering.
[0012] In step 3, in order to test the electrical properties of the ceramic sample, magnetron sputtering, firing and other methods can be used to prepare metal electrodes on both surfaces of the ceramic. First, the ceramic sample is ground and polished, and then placed in anhydrous ethanol for ultrasonic cleaning, and then dried for use. When preparing electrodes using the magnetron sputtering method, the ceramic sample is placed in the sample chamber, and the sputtering parameters are set according to the experimental conditions. After vacuuming, the sputtering coating operation can be performed. The firing electrode method is to coat the metal electrode slurry on both surfaces of the ceramic in turn through a printing operation, and dry it in an oven, and then place the sample coated with the electrode in a muffle furnace for high-temperature firing, and the preparation of the metal electrode is completed when the setting program ends.
[0013] In step 4, the ferroelectric ceramic coated with electrodes is placed in silicone oil, a certain DC or AC voltage is applied, and after pressure treatment, the flexoelectric coefficient of the ferroelectric ceramic is increased. Before the prepared sample is polarized, it is necessary to test the dielectric properties and hysteresis loop. The former is used to obtain the depolarization temperature of the sample, and the latter is used to obtain information such as the coercive electric field of the ceramic. According to the electrical properties obtained by the test, the corresponding parameters used for polarization are determined. The sample is clamped between the polarization devices, and it is ensured that the sample is completely placed in the silicone oil, and the ambient temperature of the sample is set below its depolarization temperature. Then a DC or AC voltage is applied along the thickness direction of the sample. The polarization voltage can be determined according to the hysteresis loop information of the ceramic sample to ensure that the inside of the ceramic is fully polarized as much as possible, and the holding time is selected according to the polarization of different samples, generally between 5-30 minutes. After the polarization is completed, the two sides of the sample are connected with a wire and left to stand for a period of time to eliminate the residual charge on the surface, and then the sample that has completed the polarization operation is obtained.
[0014] The flexoelectric effect uses the fact that a sample will generate a flexoelectric field when subjected to an uneven strain gradient. According to the current design ideas, this type of electrical component that can perform electromechanical conversion is mainly studied from two aspects: the macroscopic / microscopic structure design and the testing method of the sample. Considering that most excellent flexoelectric materials also have good piezoelectric properties, it is possible to try to introduce the piezoelectric effect of ferroelectric ceramics into the flexoelectric response at the same time, that is, to apply a certain voltage to the ceramic sample that originally did not require any additional electrical operations.
[0015] The test of the flexoelectric effect of the present invention adopts a point-ring test method, that is, a method of using a metal ring to support the lower surface of the sample, and using a point probe at the center of the upper surface to apply dynamic stress to cause the sample to bend. In the process of placing the sample between the clamps to apply dynamic stress, when the piezoelectric ceramic is bent, one part is stretched and the other part is compressed, and the piezoelectric responses of the two parts are offset. On the one hand, due to the continuous change of the dynamic stress in the thickness direction of the sample due to the internal polarization, a piezoelectric signal is output; on the other hand, the flexural electric field caused by the bending will also output a flexural electric signal accordingly, and the two work together; in addition, the material has non-uniformity and surface effects. Therefore, after introducing the polarization electric field into the flexoelectric test, the electromechanical response is significantly enhanced, and is much higher than the simple superposition of the two effects.
[0016] According to the method proposed in the present invention, the flexoelectric coefficient of the ferroelectric ceramic can be greatly improved by directly performing DC polarization on the ferroelectric ceramic. Here, lead zirconate titanate (PbTi x Zr 1-x O3: PZT) based ceramics are used to illustrate the feasibility of this method.
[0017] Comparative Example 1: PZT-based ceramic powder is prepared by solid phase reaction method, and the powder is formed and sintered at high temperature in a muffle furnace to obtain the desired ferroelectric ceramic. Before the electrical performance test of PZT-based ceramics, metal electrodes are prepared on both surfaces of the sample by firing method. The prepared sample is first tested by dot-ring test to obtain the flexoelectric coefficient of the unpolarized sample, which is about 2.1μC / m.
[0018] Example 1: The preparation of the sample is consistent with that of Comparative Example 1. Taking into account that different polarization operations may have different effects on the flexoelectric field, it is necessary to first determine the appropriate polarization conditions for the sample. Here, the sample is first subjected to dielectric temperature spectrum and hysteresis loop tests to determine the depolarization temperature and coercive electric field information of the sample. Then, a series of experiments on the influence of polarization on the flexoelectric effect are designed with reference to the coercive electric field and depolarization temperature of the sample, thereby determining a polarization scheme that can effectively improve the flexoelectric coefficient of ferroelectric ceramics. In order to fully polarize the ferroelectric ceramic sample, a DC or AC electric field higher than the coercive field is usually applied along the thickness direction of the sample, and the electric field is removed after being maintained for 5-30 minutes. After the sample is subjected to appropriate polarization operations, the flexoelectric coefficient of the polarized sample is measured by the point ring method, which is about 82.1μC / m.
[0019] The polarized sample was placed in a muffle furnace and depolarized by heating it above the Curie temperature. The flexoelectric coefficient of the depolarized sample was then measured by the point ring method to be approximately 0.8 μC / m.
[0020] According to the above experiments, it is determined that saturated polarized ferroelectric ceramics will show excellent improvement effects when conducting flexoelectric tests, such as Figure 1 shown. Figure 1 The flexoelectric coefficients in the figure are the test results of the same ferroelectric ceramic before and after polarization and after depolarization. By comparison, the flexoelectric coefficient of the ceramic after polarization increases by nearly 40 times, while the increase disappears after depolarization. The above results show that the polarization operation can greatly enhance the flexoelectric effect of ferroelectric ceramics, which verifies the feasibility of this technology.
Claims
1. A method for improving the flexoelectric properties of ferroelectric ceramics, characterized in that: The method comprises the following steps: Step 1, preparing ceramic powder; Step 2, preparing the synthesized ceramic powder into ferroelectric ceramics; Step 3, preparing metal electrodes on both surfaces of the ferroelectric ceramic; Step 4: placing the electrode-coated ferroelectric ceramic in silicone oil, applying a certain DC or AC electric field, and improving the flexoelectric coefficient of the ferroelectric ceramic after polarization treatment.
2. The method according to claim 1, characterized in that: In step 1, ceramic powder is synthesized by solid phase reaction; specifically, the dried raw material powder is weighed, ball-milled for 6-12 h in anhydrous ethanol as a medium, dried and placed in a crucible for calcination for 2-4 h to obtain the desired ceramic powder.
3. The method according to claim 2, characterized in that In step 2, the ceramic powder is prepared into the required ferroelectric ceramics by means of a pressing or tape casting process; the pressing is performed by adding a certain amount of polyvinyl alcohol with a mass fraction of 5% as a binder, and obtaining a ferroelectric ceramic sample by uniaxial compression or cold isostatic pressing; the tape casting is performed by adding a certain solvent to the ceramic powder and performing wet ball milling to obtain a slurry, and then scraping ferroelectric ceramic samples of different thicknesses with a scraper, removing the binder therein by high-temperature treatment, and then sintering at a corresponding temperature.
4. The method according to claim 3, characterized in that In step 3, metal electrodes are prepared on both surfaces of the sample by magnetron sputtering or sintering; specifically, the ferroelectric ceramic sample is ground, polished, and cleaned, and then the electrodes are prepared by magnetron sputtering; or the metal electrode slurry is coated on both surfaces of the ferroelectric ceramic sample and sintered at a corresponding temperature to obtain the desired sample with electrodes.
5. The method according to claim 4, characterized in that In step 4, a certain DC or AC electric field is applied along the thickness direction of the sample to polarize the sample, so as to obtain a ceramic sample with significantly improved apparent flexoelectric effect; specifically, the sample is placed in silicone oil at a temperature lower than the depolarization temperature of the sample, and a DC or AC electric field is applied along the thickness direction of the sample to fully polarize the sample; the depolarization temperature is obtained by a dielectric temperature spectrum, and the electric field is a coercive electric field obtained by a hysteresis loop test.
6. The method according to claim 5, characterized in that The applied electric field is higher than the coercive electric field and increases with the polarization saturation degree. The holding time is selected according to the polarization conditions of different samples, preferably between 5 and 30 minutes. After the polarization is completed, the two sides of the sample are connected with a wire and left to stand for a period of time to eliminate the residual charge on the surface, and then the sample that has completed the polarization operation is obtained.