Resin foam sheet and adhesive tape
By adjusting the contact angle and compression strength of the resin foam sheet, and using a multi-layer structure and specific resin materials, the lack of shear retention and flexibility of the polyolefin resin foam sheet in the adhesive tape for fixing wall hangings is solved. , achieving efficient adhesive tape performance.
Patent Information
- Application Number
- CN202380034309.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-18
- Filing Date
- 2023-04-18
- Publication Date
- 2024-11-26
AI Technical Summary
When used as an adhesive tape base material for wall hanging fixing, it is difficult to improve shear retention and flexibility at the same time, especially poor adhesion to silicone adhesives, resulting in Adhesive tape is easy to peel.
By adjusting the surface contact angle and 25% compression strength of the resin foam sheet within the specified range, combining the multi-layer structural design, using materials such as polyolefin resin and acrylic resin to form a closed-cell structure and resin film layer, and optimizing bonding The stratum structure and material composition of the belt.
When using silicone adhesive, the high shear retention force and flexibility of the resin foam sheet is achieved, ensuring the adhesion and shape of the wall surface, and extending the retention time of the adhesive tape.
Smart Images

Figure CN119032127A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resin foam sheet and a pressure-sensitive adhesive tape including the resin foam sheet. Background Art
[0002] Conventionally, foam sheets have been widely used as substrates for pressure-sensitive adhesive tapes. As the foam sheet, a polyolefin resin foam sheet obtained by foaming a foamable polyolefin resin sheet containing a thermally decomposable foaming agent is known.
[0003] In recent years, attempts have been made to make resin foam sheets multilayered in order to impart various functions. For example, Patent Document 1 discloses a multilayer foam sheet in which non-foam layers are provided on both surfaces of a foam layer in order to improve flexibility and mechanical strength. In addition, Patent Document 2 discloses a multilayer foam sheet in which outer layers consisting of foam layers having a lower foaming ratio than the middle layer are provided on both surfaces of a foam layer constituting a middle layer in order to improve reprocessability, flexibility and waterproofness.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-54961
[0007] Patent Document 2: International Publication No. 2010 / 158886 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, foam sheets are sometimes used as the base material of adhesive tapes for fixing wall hangings. Adhesive tapes for fixing wall hangings require high shear holding force so that they will not peel off from components such as the wall surface even when a shear load is applied. In addition, the foam sheet used as the base material of the adhesive tape for fixing wall hangings also requires flexibility in order to ensure the close adhesion to the wall surface, the ability to follow the shape of the wall surface, and the peelability when peeling the adhesive tape from the wall surface.
[0010] However, conventional polyolefin resin foam sheets are usually formed of polyethylene resin on the surface, but polyethylene resin is sometimes difficult to adhere to, depending on the type of adhesive such as silicone adhesive, and sometimes it is difficult to improve the shear holding force. On the other hand, if acrylic resin or the like is used in the foam sheet, the adhesion to the silicone adhesive also becomes higher, but it is difficult to form a high expansion ratio when the foam is made, and it is not easy to improve the flexibility.
[0011] Therefore, an object of the present invention is to provide a resin foam sheet which can improve both shear holding power and flexibility when used as a tape substrate of an adhesive tape using an adhesive such as a silicone-based adhesive.
[0012] Means of solving the problem
[0013] The present inventors have found that the above-mentioned problems can be solved by adjusting both the surface contact angle and the 25% compressive strength of a resin foam sheet within a predetermined range, and have completed the following invention. That is, the gist of the present invention is the following [1] to
[18] .
[0014] [1] A resin foam sheet comprising a first resin layer as a foamed resin layer, and a second resin layer which is provided on at least one surface of the first resin layer and is either a foamed resin layer or a resin film layer, wherein the contact angle of at least one surface is 36 to 95°, and the 25% compressive strength is not more than 250 kPa.
[0015] [2] The resin foam sheet according to [1] above, wherein the resin foam sheet has a thickness of 0.1 to 3.0 mm.
[0016] [3] The resin foam sheet according to [1] or [2] above, wherein the foaming ratio of the resin foam sheet is 1.5 to 20 cm 3 / g.
[0017] [4] The resin foam sheet according to any one of [1] to [3] above, which has a closed-cell structure.
[0018] [5] A resin foam sheet according to any one of [1] to [4] above, comprising a middle layer composed of the first resin layer, and an outer layer (second resin layer) respectively arranged on both sides of the middle layer and composed of either a foamed resin layer or a resin film layer.
[0019] [6] The resin foam sheet according to [5] above, wherein the foaming ratio of the outer layer is 1 to 3 cm 3 / g, and the foaming ratio of the middle layer is 3 to 20 cm 3 / g.
[0020] [7] The resin foam sheet according to [5] or [6] above, wherein the middle layer comprises a polyolefin resin, and the outer layer comprises at least one selected from the group consisting of a polyolefin resin, a modified polyolefin resin, and an acrylic resin.
[0021] [8] The resin foam sheet according to any one of [5] to [7] above, wherein the outer layers are all resin film layers.
[0022] [9] The resin foam sheet according to any one of [5] to [8] above, wherein the oxygen atom content of the two outer layers is 3.5% by mass or more.
[0023]
[10] The resin foam sheet according to any one of [1] to [9], which is used as a substrate for an adhesive tape for fixing a wall hanging.
[0024]
[11] The resin foam sheet according to any one of [1] to
[10] above, wherein the holding time in the following hanging test is 5 minutes or more.
[0025] <Suspension test>
[0026] A wall hanging having a hook is pressed onto a resin foam sheet attached to a wall surface via a silicone double-sided adhesive tape under a load of 1 kg for 5 seconds, thereby attaching the wall hanging to the resin foam sheet. Then, a 1.1 kg weight is hung on the hook of the wall hanging and the wall hanging is left to stand, and the time until the wall hanging peels off from the resin foam sheet is measured as the holding time.
[0027]
[12] The resin foam sheet according to any one of [1] to
[11] above, wherein the ratio of the thickness of each of the second resin layers to the thickness of the first resin layer (each second resin layer / first resin layer) is 0.001 to 0.5.
[0028]
[13] The resin foam sheet according to any one of [1] to
[12] above, wherein the resin constituting the first resin layer is a polyolefin resin.
[0029]
[14] The resin foam sheet according to any one of [1] to
[13] above, wherein the resin constituting the second resin layer comprises at least one selected from acrylic olefin resins, ethylene-vinyl acetate copolymers, and modified polyolefin resins.
[0030]
[15] The resin foam sheet according to [7] or
[14] above, wherein the modified polyolefin resin is an acid-modified polyolefin resin.
[0031]
[16] The resin foam sheet according to [7] or
[15] above, wherein the modified polyolefin resin is at least one selected from unsaturated carboxylic acid-modified polyethylene resins and epoxy-modified polyethylene resins.
[0032]
[17] The resin foam sheet according to [7],
[14] ,
[15] or
[16] above, wherein the modification amount based on the total amount of the second resin layer is 0.02 to 10% by mass.
[0033]
[18] A pressure-sensitive adhesive tape comprising the resin foam sheet according to any one of [1] to
[17] above, and a pressure-sensitive adhesive material located on at least one surface of the resin foam sheet.
[0034] Effects of the Invention
[0035] According to the present invention, it is possible to provide a resin foam sheet which is excellent in both shear holding power and flexibility when used as a tape substrate of an adhesive tape using various adhesives including a silicone-based adhesive. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a schematic cross-sectional view showing a resin foam sheet according to one embodiment of the present invention.
[0037] Figure 2 This is a cross-sectional schematic diagram showing an example of using a double-sided tape to fix a wall mount.
[0038] Figure 3 is a schematic cross-sectional view showing the test method of the suspension test. DETAILED DESCRIPTION
[0039] [Resin foam sheet]
[0040] The contact angle of the surface of the resin foam sheet of the present invention is 36 to 95°, and the 25% compressive strength is 250 kPa or less.
[0041] The resin foam sheet, by having the above-mentioned structure, can ensure high adhesion even when used with various adhesives including silicone adhesives, and can improve shear holding power. Therefore, even when used as a base material of an adhesive tape for fixing wall-mounted parts and subjected to a high shear load, it can prevent peeling from the wall surface, etc. In addition, high flexibility can be ensured, for example, it can also ensure adhesion to the wall surface, flexibility to the wall surface shape, and peelability when peeling the adhesive tape from the wall surface.
[0042] <Contact angle>
[0043] The contact angle of the surface of the resin foam sheet of the present invention is 36 to 95°. If the contact angle is greater than 95°, the wettability to silicone adhesives and the like sometimes deteriorates, and the adhesion to the adhesive deteriorates. Therefore, if a high shear load is applied to an adhesive tape with the resin foam sheet as a substrate, the adhesive is easily peeled off from the resin foam sheet, causing the adherend to peel off together with the adhesive, or the adhesive remains on the adherend, causing the resin foam sheet to peel off from the adhesive, thereby causing the adhesive tape to fall off. In addition, if the contact angle is less than 36°, it is difficult to manufacture the resin foam sheet in a practical manner.
[0044] From the above viewpoints, the contact angle is preferably 50° or more, more preferably 60° or more, and further preferably 80° or more. The contact angle is preferably 93° or less, and further preferably 91° or less.
[0045] It should be noted that, as described later, the contact angle can be appropriately adjusted according to the type of resin used in the resin foam sheet, and more specifically, can be adjusted by appropriately selecting the type of resin used in the second resin layer (outer layer). That is, the surface of the resin foam sheet preferably composed of the second resin layer (outer layer) described later can reach the range of the contact angle as described above.
[0046] In addition, the resin foam sheet, the contact angle of at least any foam sheet surface is within the above range, but the contact angles of the two faces of the preferred foam sheet are all within the above range. When the contact angles of the two faces of the foam sheet are within the above range, it can be suitable for use as the base material of the double-sided adhesive tape. As described in the examples, the contact angle is the contact angle relative to pure water.
[0047] <25% compression strength>
[0048] The 25% compressive strength of the resin foam sheet of the present invention is 250 kPa or less. When the 25% compressive strength is greater than 250 kPa, the flexibility of the resin foam sheet decreases, which may reduce the adhesion to the adherend such as the wall surface, the followability to the wall surface shape, and the peelability when peeling the adhesive tape from the adherend such as the wall surface.
[0049] From the perspective of further improving the flexibility of the resin foam sheet, the 25% compressive strength of the resin foam sheet of the present invention is preferably 200 kPa or less, more preferably 150 kPa or less, and further preferably 90 kPa or less. In addition, the 25% compressive strength of the resin foam sheet is not particularly limited, but from the perspective of imparting a certain mechanical strength to the resin foam sheet, it is preferably 10 kPa or more, and more preferably 20 kPa or more.
[0050] <Closed-cell structure>
[0051] The resin foam sheet of the present invention preferably has a closed-cell structure. The resin foam sheet can improve the shear strength while ensuring flexibility by having a closed-cell structure, and can easily improve the shear holding power.
[0052] It should be noted that the closed-cell structure means that the bubbles in the resin foam sheet are generally independent bubbles, and the closed-cell ratio of the resin foam sheet is, for example, 70% or more, preferably 80% or more, more preferably 90% or more, and further preferably 92% or more. The upper limit of the closed-cell ratio is not particularly limited and is 100%. It should be noted that the closed-cell ratio can be measured by the method described in the examples.
[0053] <Thickness>
[0054] The thickness of the resin foam sheet is preferably 0.1 to 3 mm. If the thickness of the resin foam sheet is within the above range, it is easy to make the flexibility and mechanical strength of the resin foam sheet good. In addition, it is possible to fully ensure the thickness required as an adhesive tape substrate, especially an adhesive tape substrate for fixing wall hangings, and it is also possible to prevent the tape substrate from becoming thicker than necessary. From this aspect, the thickness of the resin foam sheet is more preferably 0.3 to 2 mm, and more preferably 0.5 to 1.6 mm.
[0055] <Foaming ratio>
[0056] The foaming ratio of the resin foam sheet of the present invention is preferably 1.5 to 20 cm 3 / g. By setting the expansion ratio to 1.5 cm 3 / g or more, the softness of the resin foam sheet is improved, and the above-mentioned 25% compressive strength is easily reduced. In addition, by setting the foaming ratio to 20 cm 3 / g or less, the mechanical strength of the resin foam sheet is improved, and the above-mentioned shear holding force and the like are also easily improved. The foaming ratio of the resin foam sheet is more preferably 5 to 19 cm 3 / g, more preferably 10 to 18 cm 3 / g.
[0057] It should be noted that the expansion ratio is expressed as the reciprocal of the apparent density, and the expansion ratio of the resin foam sheet can be determined by measuring the apparent density of the entire resin foam sheet and finding its reciprocal. The apparent density can be measured in accordance with JIS K7222.
[0058] <Retention time>
[0059] The resin foam sheet of the present invention is preferably held for 5 minutes or more in the following hanging test. If the holding time is 5 minutes or more, the resin foam sheet of the present invention is not likely to peel off even when used as a wall hanging fixture.
[0060] <Suspension test>
[0061] A wall hanging piece having a hook is pressed onto a resin foam sheet attached to a wall surface through a silicone double-sided adhesive tape under a load of 1 kg for 5 seconds, thereby attaching the wall hanging piece to the resin foam sheet. Then, a 1.1 kg weight is hung on the hook of the wall hanging piece and the wall hanging piece is left to stand, and the time until the wall hanging piece is peeled off from the resin foam sheet is measured as the retention time.
[0062] <Layer Structure of Resin Foam Sheet>
[0063] The resin foam sheet at least comprises a foamed resin layer formed of a foam body. In the present invention, the resin foam sheet comprises a foamed resin layer (hereinafter, sometimes referred to as a first resin layer) and an outer layer (hereinafter, sometimes referred to as a second resin layer) provided on at least one side of the foamed resin layer. Figure 1 As shown, the resin foam sheet is preferably a resin foam sheet 10 having a middle layer (first resin layer) 11 composed of a foamed resin layer and outer layers (second resin layers) 12A and 12B respectively arranged on both surfaces of the middle layer 11. The resin foam sheet 10 can easily adjust the contact angles of the two surfaces to a desired range by providing the outer layers 12A and 12B. It should be noted that in the resin foam sheet, the outer layer (second resin layer) can be a layer constituting the surface of the resin foam sheet.
[0064] The outer layer is any one of a resin film layer and a foamed resin layer. Here, the foamed resin layer is a layer composed of a foam body, and the resin film layer is a layer composed of a non-foam body. The outer layers 12A and 12B may be both resin film layers, both foamed resin layers, or one may be a resin film layer and the other may be a foamed resin layer. Among them, it is preferred that the two outer layers 12A and 12B are resin film layers. By making the two outer layers 12A and 12B resin film layers, the shear holding force is easily increased, and even if used as a tape base material for fixing a wall hanging, it is not easy to cause undesirable conditions such as peeling.
[0065] (Expansion ratio of the first resin layer and the second resin layer)
[0066] In the resin foam sheet, the foaming ratio of the first resin layer (middle layer) is preferably 3 to 20 cm 3 / g. By making the foaming ratio of the first resin layer 3cm 3 / g or more, the softness of the resin foam sheet is improved, and the above-mentioned 25% compressive strength is easily reduced. In addition, by making the foaming ratio 20cm 3 / g or less, the mechanical strength of the resin foam sheet is improved. The foaming ratio of the resin foam sheet is more preferably 6 to 19 cm 3 / g, more preferably 10 to 18 cm 3 / g.
[0067] It is preferred that the foaming ratio of each second resin layer (outer layer) is lower than that of the first resin layer (middle layer). By making the foaming ratio of the second resin layer lower than that of the first resin layer, it is easy to ensure the mechanical strength of the resin foam sheet. From the perspective of easily ensuring the mechanical strength and shear strength of the resin foam sheet, the foaming ratio of the second resin layer is preferably 1 to 3 cm 3 / g, more preferably 1 to 2 cm 3 / g, more preferably 1 to 1.5 cm 3 / g.
[0068] It should be noted that the expansion ratio of the first resin layer and the second resin layer can be determined by measuring the apparent density of each layer and finding its inverse. Therefore, the second resin layer is sometimes a non-foamed body. Even in such a case, the second resin layer should have a foaming ratio. It should be noted that the foaming ratio of a non-foamed body is approximately 1 cm 3 / g.
[0069] (Thickness of the First Resin Layer and the Second Resin Layer)
[0070] The thickness of the first resin layer (middle layer) in the resin foam sheet is preferably 0.05 to 2.9 mm. When the thickness of the first resin layer is within the above range, it is easy to ensure flexibility. In addition, the thickness required as an adhesive tape substrate, especially an adhesive tape substrate for fixing wall hangings, can be fully ensured, and the tape substrate can be prevented from becoming thicker than necessary. From this aspect, the thickness of the first resin layer is more preferably 0.25 to 1.9 mm, and more preferably 0.4 to 1.5 mm.
[0071] The thickness of each second resin layer (outer layer) is preferably 3 to 300 μm. If the thickness of the second resin layer is 3 to 300 μm, it is easy to improve the adhesion to various adhesives such as silicone adhesives while ensuring a certain mechanical strength and flexibility. From this aspect, the thickness of each second resin layer is more preferably 5 to 200 μm, more preferably 10 to 100 μm, and even more preferably 15 to 70 μm.
[0072] The thickness ratio of each second resin layer (outer layer) to the first resin layer (middle layer) (each second resin layer / first resin layer) is preferably 0.001 to 0.5. If the thickness ratio is within the above range, it is easy to ensure the flexibility and mechanical strength of the resin foam sheet while also making it easy to make the adhesion to various adhesives such as silicone adhesives good. The above thickness ratio is more preferably 0.005 to 0.4, further preferably 0.01 to 0.3, and further preferably 0.015 to 0.15.
[0073] (oxygen atom content)
[0074] The resin foam sheet preferably has an oxygen atom content of 3.5% by mass or more in the second resin layer (outer layer). By making the oxygen atom content 3.5% by mass or more, the adhesion to various adhesives such as silicone adhesives becomes good, and the shear holding force of the adhesive tape becomes good. From the perspective of achieving good adhesion to silicone adhesives, the above oxygen atom content is more preferably 4% by mass or more, and further preferably 6% by mass or more. In addition, the above oxygen atom content is not particularly limited, for example, it is 15% by mass or less.
[0075] As described below, the oxygen atom content can be appropriately adjusted by the type of resin used in the resin foam sheet, and preferably can be adjusted by appropriately selecting the type of resin used in the outer layer described below.
[0076] The resin foam sheet preferably has at least one outer layer with an oxygen atom content within the above range, and preferably has both outer layers with oxygen atom contents within the above range. When both outer layers have oxygen atom contents within the above range, the sheet can be suitably used as a substrate for a double-sided adhesive tape.
[0077] (Composition of the first resin layer)
[0078] In the resin foam sheet of the present invention, the foamed resin layer is formed of a foam. The type of resin constituting the foamed resin layer is not particularly limited, and any known resin used as a foam may be used.
[0079] As mentioned above, the first resin layer is composed of a foamed resin layer. From the perspective of flexibility and processability, the resin constituting the first resin layer (middle layer) is preferably a thermoplastic resin, more preferably a polyolefin resin. By using a polyolefin resin, while ensuring flexibility, it is easy to improve shear strength, and shear holding power, etc. are also easy to become good. The polyolefin resin can be a polyolefin resin such as a polyethylene resin and a polypropylene resin, or it can be an olefin copolymer resin such as an ethylene-vinyl acetate copolymer, etc., wherein, from the perspective of flexibility and shear strength, a polyethylene resin is preferred.
[0080] Examples of the polyethylene resin include polyethylene resins polymerized using a polymerization catalyst such as a Ziegler-Natta compound, a metallocene catalyst, and a chromium oxide compound. Preferably, a polyethylene resin polymerized using a metallocene catalyst is used.
[0081] (Metallocene Catalyst)
[0082] Examples of metallocene catalysts include compounds such as bis(cyclopentadienyl) metal complexes having a structure in which a transition metal is sandwiched between π-electron unsaturated compounds. More specifically, examples include compounds in which one or more cyclopentadienyl rings or their analogs exist as ligands on a tetravalent transition metal such as titanium, zirconium, nickel, palladium, hafnium, and platinum.
[0083] The properties of the active points of the metallocene catalyst are uniform, and each active point has the same degree of activity. Since the molecular weight, molecular weight distribution, composition, composition distribution, etc. of the polymer synthesized using the metallocene catalyst are highly uniform, when a sheet containing a polymer synthesized using the metallocene catalyst is cross-linked, the cross-linking can be performed uniformly. The uniformly cross-linked sheet can be uniformly foamed, so it is easy to stabilize the physical properties. In addition, since it can be uniformly stretched, the thickness of the foam can be made uniform.
[0084] As the ligand, for example, a cyclopentadienyl ring, an indenyl ring, etc. can be cited. These cyclic compounds can be substituted by a hydrocarbon group, a substituted hydrocarbon group, or a hydrocarbon-substituted metalloid group. As the hydrocarbon group, for example, a methyl group, an ethyl group, various propyl groups, various butyl groups, various pentyl groups, various hexyl groups, 2-ethylhexyl groups, various heptyl groups, various octyl groups, various nonyl groups, various decyl groups, various cetyl groups, phenyl groups, etc. can be cited. It should be noted that "various" refers to various isomers including normal, secondary, tertiary, and iso.
[0085] Furthermore, a ligand obtained by polymerizing a cyclic compound into an oligomer may be used.
[0086] In addition to the π-electron unsaturated compounds, monovalent anionic ligands such as chlorine and bromine or divalent anionic chelating ligands, hydrocarbons, alcohol salts, arylamide, aryloxide, amide, arylamide, phosphide, arylphosphide, etc. can also be used.
[0087] Examples of the metallocene catalyst containing a tetravalent transition metal and a ligand include cyclopentadienyl titanium tris(dimethylamide), methylcyclopentadienyl titanium tris(dimethylamide), bis(cyclopentadienyl)titanium dichloride, and dimethylsilyltetramethylcyclopentadienyl-tert-butylamide zirconium dichloride.
[0088] Metallocene catalysts act as catalysts in the polymerization of various olefins by combining with specific co-catalysts (co-catalysts). Specific co-catalysts include methylaluminoxane (MAO), boron compounds, etc. It should be noted that the ratio of the co-catalyst to the metallocene catalyst is preferably 100,000 to 1,000,000 mole times, and more preferably 500,000 to 5,000 mole times.
[0089] Examples of polyethylene resins include low-density polyethylene (LDPE: density 0.925 g / cm 3 Below), medium density polyethylene (MDPE: density exceeding 0.925g / cm 3 And 0.945g / cm 3 Below), high-density polyethylene (HDPE: density exceeding 0.945g / cm 3 ), linear low-density polyethylene (LLDPE), among which linear low-density polyethylene is preferred.
[0090] As a linear low-density polyethylene, a linear low-density polyethylene obtained by copolymerizing ethylene (for example, 75% by mass or more, preferably 90% by mass or more relative to the total monomer amount) with a small amount of α-olefin as required is more preferred. As α-olefins, specifically, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-octene can be cited. Among them, α-olefins with a carbon number of 4 to 10 are preferred.
[0091] From the viewpoint of flexibility, the density of the linear low-density polyethylene is preferably 0.870 to 0.925 g / cm 3 , more preferably 0.890 to 0.925 g / cm 3 , more preferably 0.910 to 0.925 g / cm 3 As the polyethylene resin, one type may be used alone, or a plurality of types of polyethylene resins may be used.
[0092] Preferably, the polyolefin resin is used as the main component in the first resin layer (middle layer), and the specific content of the polyolefin resin is, for example, 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more, based on the total amount of resin contained in the first resin layer. In addition, in the foamed resin layer constituting the first resin layer, as a resin component, the polyolefin resin alone may be used, but as long as the effect of the present invention is not impaired, a resin other than the polyolefin resin may also be contained.
[0093] (Composition of the Second Resin Layer)
[0094] As mentioned above, the second resin layer (outer layer) is a resin film layer or a foamed resin layer. The type of resin constituting the second resin layer is not particularly limited, and a resin having a surface contact angle reaching the above range can be selected. In addition, from the processability aspect, the resin used in each second resin layer is preferably a thermoplastic resin, but may also be a curable resin such as a thermosetting resin or a photocurable resin.
[0095] As the resin used in each second resin layer (outer layer), modified polyolefin resins such as polyolefin resins, acid-modified polyolefin resins, and acrylic resins can be listed. These resins can be used alone or in combination of two or more. By using these resins in the second resin layer, the contact angle of the surface of the resin foam sheet can be easily adjusted to within a specified range.
[0096] It should be noted that, as described above, the second resin layers are preferably provided on both surfaces of the middle layer, and the resins contained in the plurality of second resin layers may be the same as or different from each other.
[0097] As the polyolefin resin used in the second resin layer, an olefin copolymer resin which is a copolymer of an olefin and a monomer other than an olefin such as vinyl acetate or (meth) acrylic acid ester is preferably used. The olefin used in the olefin copolymer resin is, for example, an α-olefin having a carbon number of about 2 to 12 such as ethylene, propylene, butene, and methylpentene-1, preferably ethylene. As the olefin copolymer resin, acrylic olefin resins and ethylene vinyl acetate copolymers are preferably mentioned.
[0098] Preferred specific examples of acrylic olefin resins include acrylic ethylene resins such as ethylene-ethyl acrylate copolymer (EEA), ethylene-methyl acrylate copolymer (EMA), ethylene-butyl acrylate copolymer (EBA), and ethylene-methyl methacrylate copolymer (EMMA).
[0099] By using the above olefin copolymer resin in the second resin layer, the contact angle of the surface of the resin foam sheet can be appropriately adjusted, and the oxygen atom content can be easily adjusted to a desired range. Among them, acrylic olefin resins are preferred, and acrylic ethylene resins are more preferred.
[0100] Examples of modified polyolefin resins include acid-modified polyolefin resins modified with at least one of unsaturated carboxylic acid and its anhydride, specifically, polyolefin resins in which unsaturated carboxylic acid or the like is chemically bonded to the polyolefin resin by addition reaction, graft reaction or the like.
[0101] Examples of the unsaturated carboxylic acid used to modify the acid-modified polyolefin resin include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, and anhydrides thereof. Among them, maleic acid or anhydride thereof is preferred.
[0102] The modified polyolefin resin is not limited to the acid-modified resin such as the carboxylic acid-modified resin described above, which acts as a Bronsted acid, but may be a resin other than the acid-modified resin, such as a resin that acts as a Bronsted base.
[0103] As the resin to which the Bronsted base acts, a resin containing an epoxy group is preferred. Therefore, the modified polyolefin resin is also preferably an epoxy group-modified polyolefin resin.
[0104] As polyolefin resins, for example, homopolymers or copolymers of α-olefins having a carbon number of about 2 to 12, such as ethylene, propylene, butene, and methylpentene-1, can be cited. Among them, polyethylene resins and polypropylene resins are preferred, and polyethylene resins are preferred. Therefore, the modified polyolefin resin is preferably a modified polyethylene resin. In addition, the acid-modified polyolefin resin is preferably an acid-modified polyethylene resin. In addition, the acid-modified polyolefin resin may contain structural units derived from components other than olefins and unsaturated carboxylic acids and their anhydrides, and may contain structural units derived from vinyl acetate and various (meth)acrylates.
[0105] The modified polyolefin resin such as the acid-modified polyolefin resin may contain a structural unit derived from an olefin as a main component, and may contain 50% by mass or more, preferably 60% by mass or more, and more preferably 70% by mass or more of the olefin based on the total monomer amount.
[0106] Examples of the acid-modified polyolefin resin include resins obtained by graft-copolymerizing at least one of an unsaturated carboxylic acid and an anhydride thereof with a polyolefin resin such as a polyethylene resin.
[0107] In addition, copolymers of olefins such as ethylene and unsaturated carboxylic acids or their anhydrides such as maleic anhydride, maleic acid, (meth)acrylic acid, and other components used as needed may be mentioned. In this case, maleic anhydride is preferred as the unsaturated carboxylic acid or its anhydride.
[0108] Examples of epoxy-modified polyethylene resins include copolymers of olefins such as ethylene, epoxy-containing compounds such as glycidyl (meth)acrylate, and other components as needed.
[0109] Specific examples of preferred modified polyolefin resins include unsaturated carboxylic acid-modified polyethylene resins such as maleic anhydride-modified polyethylene resins, maleic acid-modified polyethylene resins, (meth)acrylic acid-modified polyethylene resins, and epoxy-modified polyethylene resins. As modified polyolefin resins, unsaturated carboxylic acid-modified polyethylene resins are preferred from the perspective of improving shear holding power, and specifically, maleic anhydride-modified polyethylene resins and maleic acid-modified polyethylene resins are more preferred, and maleic anhydride-modified polyethylene resins are particularly preferred.
[0110] The modification amount of the modified polyolefin resin (the acid modification amount in the modified polyolefin resin) is not particularly limited, and is, for example, 0.1 to 25% by mass, preferably 0.5 to 20% by mass, and more preferably 1 to 15% by mass. It should be noted that the modification amount herein is represented by the mass % of the structural unit derived from the monomer containing a modifying group such as an unsaturated carboxylic acid or an epoxy-containing compound in the modified polyolefin resin.
[0111] The acrylic resin used in the second resin layer may be an acrylic polymer formed by polymerizing a monomer component (a) containing an acrylic monomer component. The monomer component (a) is a monomer component having one addition polymerizable double bond, preferably a monomer component having one vinyl group. The monomer component (a) is not particularly limited, but preferably contains an alkyl (meth)acrylate as the acrylic monomer component.
[0112] It should be noted that, in the present specification, (meth)acrylate means acrylate or methacrylate, and other similar terms are the same.
[0113] Examples of the alkyl (meth)acrylate include alkyl (meth)acrylates having a linear or branched alkyl group, and the alkyl group has, for example, 1 to 18 carbon atoms, preferably 1 to 14 carbon atoms, more preferably 1 to 10 carbon atoms, and further preferably 1 to 8 carbon atoms.
[0114] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-undecyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, and n-tetradecyl (meth)acrylate.
[0115] In the monomer component (a) constituting the acrylic polymer, the (meth) alkyl acrylate preferably contains 50% by mass or more, more preferably 60% by mass or more and 100% by mass or less, further preferably 75% by mass or more and 100% by mass or less, and further preferably 90% by mass or more and 100% by mass or less. By using the (meth) alkyl acrylate above these lower limits, it is easy to give the foaming resin layer the required mechanical strength, etc. In addition, the monomer component (a) can also be entirely (meth) alkyl acrylate.
[0116] In addition, the monomer component (a) may contain monomer components other than the alkyl (meth)acrylate in addition to the above-mentioned alkyl (meth)acrylate. Examples of monomer components other than the alkyl (meth)acrylate include carboxyl-containing monomers or their anhydrides, hydroxyl-containing (meth)acrylic acid monomers, nitrogen-containing vinyl monomers, styrene-based monomers, and the like.
[0117] Examples of the carboxyl group-containing monomer include carboxylic acids containing an addition polymerizable double bond, such as (meth)acrylic acid, crotonic acid, cinnamic acid, itaconic acid, maleic acid, fumaric acid, and citraconic acid.
[0118] Examples of the hydroxyl group-containing (meth)acrylic acid monomer include hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone-modified (meth)acrylate, polyoxyethylene (meth)acrylate, and polyoxypropylene (meth)acrylate.
[0119] Examples of the nitrogen-containing vinyl monomer include acrylamides such as (meth)acrylamide, N-methyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-ethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N-propyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, N-butyl (meth)acrylamide, and N,N-dibutyl (meth)acrylamide; (meth)acrylic acid monomers containing an amino group such as aminoethyl (meth)acrylate and tert-butylaminoethyl (meth)acrylate; (meth)acrylonitrile; N-vinyl pyrrolidone, N-vinyl caprolactam, N-vinyl laurolactam, (meth)acryloyl morpholine, and dimethylaminomethyl (meth)acrylate.
[0120] Examples of the styrene-based monomers include styrene, α-methylstyrene, o-methylstyrene, and p-methylstyrene.
[0121] The monomer components other than the (meth)acrylic acid alkyl ester may be used alone or in combination of two or more.
[0122] The acrylic polymer may be cross-linked by a cross-linking agent to have a cross-linked structure. When the acrylic polymer is cross-linked by a cross-linking agent, for example, during the polymerization of the monomer component (a), the cross-linking agent is further added to copolymerize the monomer component (a) and the cross-linking agent, thereby cross-linking the acrylic polymer by the cross-linking agent. Alternatively, the acrylic polymer may be cross-linked by the cross-linking agent by adding a cross-linking agent to a substance formed by partially polymerizing the monomer component (a) and further polymerizing the substance.
[0123] As the crosslinking agent, there can be mentioned a crosslinking agent having two or more addition polymerizable double bonds, preferably a crosslinking agent having two or more vinyl groups, and more preferably a multifunctional (meth)acrylate having two or more (meth)acryloyl groups. Such a crosslinking agent is introduced into the main chain composed of the monomer component (a), and the main chains are crosslinked to form a network.
[0124] Specific examples of the crosslinking agent include hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, ε-caprolactone-modified tris(2-acryloyloxyethyl)isocyanurate, caprolactone-modified ethoxylated isocyanuric acid triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, propoxylated glycerol triacrylate, neopentyl glycol adipate diacrylate, polyurethane acrylate, epoxy acrylate, polyester acrylate, and liquid hydrogenated 1,2-polybutadiene diacrylate. The crosslinking agent may be used alone or in combination of two or more.
[0125] The amount of the crosslinking agent is preferably 0.5 to 10 parts by mass, more preferably 1 to 8 parts by mass, and even more preferably 2 to 6 parts by mass, based on 100 parts by mass of the monomer component (a).
[0126] As the resin used in each second resin layer, among the above resins, a resin selected from olefin copolymer resins, modified polyolefin resins and acrylic resins is preferred from the viewpoint of easy adjustment of the contact angle to a desired range. Among them, when the first resin layer (middle layer) contains an olefin resin, from the viewpoint of adhesion to the first resin layer, an olefin copolymer resin and an acid-modified polyolefin resin are more preferred, and an acid-modified polyolefin resin is further preferred.
[0127] These resins may be used alone or in combination of two or more.
[0128] In addition, it is preferred that the resin selected from the group consisting of olefin copolymer resins, modified polyolefin resins and acrylic resins is used as the main component in each second resin layer, preferably containing 50% by mass or more, more preferably 70% by mass or more, and further preferably 90% by mass or more, based on the total amount of the second resin layer. In addition, in each second resin layer, the resin selected from these may be used in combination with other resins, for example, it may be used in combination with a polyolefin resin other than an olefin copolymer resin or a modified polyolefin resin.
[0129] In addition, when a modified polyolefin resin is used in the second resin layer, the modified polyolefin resin does not need to be the main component, and the content can be appropriately adjusted in a manner that the modified amount reaches a certain range. Specifically, the second resin layer is made to contain a modified polyolefin resin in a manner such as 0.02 to 10% by mass, preferably 0.05 to 8% by mass, more preferably 0.1 to 6% by mass, and further preferably 0.2 to 6% by mass, based on the modified amount of the second resin layer total amount. It should be noted that the modified amount based on the second resin layer total amount refers to the ratio (mass %) of the structural units containing modified group monomers such as unsaturated carboxylic acids and epoxy-containing compounds relative to the total amount of the second resin layer. The modified amount based on the second resin layer total amount can be calculated by the amount of each component, or it can be obtained by, for example, measuring the surface of the resin foam sheet with XPS.
[0130] When a modified polyolefin resin is used in the second resin layer, a polyolefin resin can be cited as a resin used in combination with the modified polyolefin resin. As the polyolefin resin, it can be a polyolefin resin such as a polyethylene resin and a polypropylene resin, or it can be an olefin copolymer resin such as an ethylene-vinyl acetate copolymer, preferably a polyethylene resin. The details of the polyethylene resin used in the second resin layer are as described in the first resin layer above, so its description is omitted. It should be noted that for the polyolefin resin used in combination with the modified polyolefin resin in the second resin layer, a polyolefin resin of a different type from the polyolefin resin used in the first resin layer can be used, but it is preferred to use the same type. Therefore, if the resin used in the first resin layer is a polyethylene resin, the resin used in combination with the modified polyolefin resin in the second resin layer is also preferably a polyethylene resin. In addition, if the resin used in the first resin layer is LLDPE, the resin used in combination with the modified polyolefin resin in the second resin layer is also preferably LLDPE.
[0131] When a modified polyolefin resin is used in the second resin layer, the content of the modified polyolefin resin in the second resin layer is, for example, 5 to 100 mass %, preferably 10 to 100 mass %, and more preferably 15 to 40 mass % based on the total mass of the second resin layer.
[0132] (foaming agent)
[0133] The foamed resin layer is preferably obtained by foaming a foamed resin layer comprising the above-mentioned resin and a foaming agent with a foamable composition. As the foaming agent, a thermal decomposition type foaming agent is preferred. When the foamed resin layer contains additives, various additives can be further formulated in the foamable composition.
[0134] As the thermal decomposition type foaming agent, an organic foaming agent or an inorganic foaming agent can be used. Examples of the organic foaming agent include azodicarbonamide, azodicarboxylic acid metal salts (barium azodicarboxylate, etc.), azo compounds such as azobisisobutyronitrile, nitroso compounds such as N,N'-dinitrosopentamethylenetetramine, biurea, 4,4'-oxybis(benzenesulfonylhydrazide), hydrazine derivatives such as toluenesulfonylhydrazide, and semicarbazide compounds such as toluenesulfonylsemicarbazide.
[0135] Examples of the inorganic foaming agent include ammonium carbonate, sodium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate.
[0136] Among them, from the viewpoint of obtaining fine bubbles, economic efficiency and safety, azo compounds are preferred, and azodicarbonamide is more preferred.
[0137] The thermal decomposition type foaming agent may be used alone or in combination of two or more.
[0138] The amount of the foaming agent in the foamable composition for the foamed resin layer can be appropriately adjusted according to the desired foaming ratio. For example, in the foamable composition for the foamed resin layer used to form the first resin layer, the content of the foaming agent is preferably 1 to 20 parts by mass, more preferably 3 to 18 parts by mass, and further preferably 5 to 15 parts by mass relative to 100 parts by mass of the resin. By making the amount of the foaming agent above these lower limits, the flexibility of the resin foam sheet is improved. In addition, by making the amount of the foaming agent below these upper limits, the first resin layer can be prevented from being excessively foamed, so that the mechanical strength of the resin foam sheet is good.
[0139] In addition, in the foamable composition for the foamed resin layer constituting the second resin layer, the content of the foaming agent is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and further preferably 1 to 3 parts by mass relative to 100 parts by mass of the resin. By making the amount of the foaming agent above these lower limits, the foaming ratio of the second resin layer can be made above a certain value. In addition, by making the amount of the foaming agent below these upper limits, excessive foaming of the foam can be prevented, so that the mechanical strength of the resin foam sheet is good.
[0140] As described above, the second resin layer is preferably a resin film layer (ie, a non-foamed body), and therefore, the second resin layer is preferably formed of a resin composition that does not contain a foaming agent.
[0141] (additive)
[0142] The resin foam sheet may contain additives in addition to the resin component. As additives, additives that can be used for foams and resin films in the past can be listed, for example, antioxidants, colorants, flame retardants, antistatic agents, fillers, ultraviolet absorbers, decomposition temperature regulators, photopolymerization initiators, crosslinking agents, etc. In addition, as described above, the resin foam sheet preferably has a first resin layer and a second resin layer, and the first resin layer and the second resin layer each contain additives appropriately.
[0143] The resin foam sheet preferably contains the above-mentioned antioxidant. When the resin foam sheet is composed of multiple layers, the antioxidant can be contained in each layer. For example, when the resin foam sheet has a first resin layer and a second resin layer, the first resin layer and the second resin layer can each contain an antioxidant. Examples of the antioxidant include phenolic antioxidants such as 2,6-di-tert-butyl-p-cresol, sulfur antioxidants, phosphorus antioxidants, and amine antioxidants.
[0144] The content of the antioxidant in each layer is, for example, 0.01 to 5 parts by mass relative to 100 parts by mass of the resin contained in each layer.
[0145] In addition, the foamable composition (i.e., the foamed resin layer) may contain a decomposition temperature regulator. The decomposition temperature regulator is a substance added as a substance to lower the decomposition temperature of the thermal decomposition type foaming agent or to accelerate the decomposition rate for regulation. Specific compounds include zinc oxide, zinc stearate, urea, etc. The decomposition temperature regulator is added in each foamed resin layer, for example, in an amount of 0.01 to 5 parts by mass relative to 100 parts by mass of the resin.
[0146] (Adhesive layer)
[0147] In the resin foam sheet, it is preferred that the second resin layer (outer layer) is directly laminated with the first resin layer (middle layer), but it is also possible to laminate with other layers. As other layers, for example, an adhesive layer can be cited. As the adhesive layer, known adhesives, adhesives, etc. can be used. In addition, it is also possible to have a double-sided adhesive tape with adhesive layers on both sides of the substrate.
[0148] It should be noted that the adhesive layer can have a thickness that does not significantly affect physical properties such as mechanical strength and flexibility in the resin foam sheet. Therefore, the thickness of the adhesive layer that bonds the outer layer and the foamed resin layer is preferably thinner than the outer layer, and more preferably less than 1 / 2 of the thickness of the outer layer.
[0149] <Method for producing resin foam sheet>
[0150] The manufacturing method of the resin foam sheet is not particularly limited. In the case of obtaining a multilayer resin foam sheet, a multilayer sheet can be obtained by laminating a plurality of resin layers, and then at least one layer of the resin layer in the multilayer sheet is foamed to obtain a method (hereinafter, also referred to as "manufacturing method 1") to manufacture.
[0151] More specifically, the production method 1 includes the following steps I and II.
[0152] (I) a step of obtaining a multilayer sheet having a layer formed of a foamable composition for forming a first resin layer and a layer for forming a second resin layer,
[0153] (II) A step of obtaining a foamed resin sheet by foaming the multilayer sheet.
[0154] Hereinafter, each step will be described.
[0155] (Step (I))
[0156] As a method for obtaining a multilayer sheet in operation (I), there is no particular restriction, and it is preferably carried out by coextrusion. Specifically, the resin, thermal decomposition type foaming agent and other foaming agents used to form the first resin layer (middle layer) and the additives matched as needed are supplied to an extruder for melt mixing to obtain a resin composition (foamable composition) for the first resin layer. In addition, the resin used to form the second resin layer (outer layer) and other foaming agents and additives matched as needed are supplied to other extruders for melt mixing to obtain a resin composition for the second resin layer. Then, the resin composition supplied from each extruder is confluent, and is extruded into a sheet using a T-die, so that a multilayer sheet can be obtained. Coextrusion can be any one of a feed block method and a multi-manifold method, preferably a feed block method.
[0157] The multilayer sheet obtained in step (I) may be provided with a layer for forming the first resin layer and a layer for forming the second resin layer, and is preferably a multilayer sheet in which layers for forming the second resin layer are laminated on both sides of the layer for forming the first resin layer. In addition, the layer for forming the second resin layer may be a layer formed of a foamable composition having a foaming agent, or a layer formed of a resin composition not having a foaming agent.
[0158] In step (I), the multilayer sheet obtained above is preferably further crosslinked. As a crosslinking method, there is a method of pre-mixing an organic peroxide as a crosslinking agent and heating the multilayer sheet obtained in step (I) to crosslink, but a method of irradiating the multilayer sheet with ionizing radiation to crosslink is preferred. It should be noted that examples of ionizing radiation include electron beams, β rays, etc., and electron beams are preferred.
[0159] The irradiation dose of ionizing radiation is preferably 1 to 10 Mrad, more preferably 1.5 to 5 Mrad.
[0160] (Step (II))
[0161] In step (II), the multilayer sheet obtained in step (I) is subjected to a foaming treatment to foam the layer formed of the foamable composition. The layer formed of the foamable composition may be treated in a manner that the foaming agent is foamed. However, when the foaming agent is a thermally decomposable foaming agent, the multilayer sheet is heated to foam. The heating temperature may be above the temperature at which the thermally decomposable foaming agent decomposes, for example, about 150 to 320°C.
[0162] The method for heating the multilayer sheet is not particularly limited, and examples thereof include a method of heating the multilayer sheet using hot air, a method of heating using infrared rays, a method of heating using a salt bath, a method of heating using an oil bath, etc., and these methods may be used in combination.
[0163] The multilayer sheet may be appropriately stretched while being foamed, or appropriately stretched after being foamed.
[0164] In step (II), the layer for forming the first resin layer may be foamed. However, when the layer for forming the second resin layer is a foamable composition, the second resin layer may also be foamed together.
[0165] (Second Manufacturing Method)
[0166] The multilayer resin foam sheet can also be manufactured by other methods. Specifically, a method (also referred to as "the second manufacturing method") can be cited in which a foamed body constituting the first resin layer is pre-manufactured, a resin film or a foamed body (outer layer) is superimposed on one or both sides of the foamed body (the first resin layer) and bonded.
[0167] As a method for obtaining a foam in the second manufacturing method, the resin, the thermal decomposition type foaming agent and the additives prepared as required for forming the foamed resin layer can be melt-kneaded to obtain a foamable composition for the foamed resin layer, and the foamable composition is molded into a sheet (foamable composition sheet). The method of melt-kneading the foamable composition to be molded into a sheet is not particularly limited, and is preferably carried out using an extruder.
[0168] The obtained foamable composition sheet is preferably further crosslinked before foaming as described below. As a crosslinking method, there is a method of pre-mixing an organic peroxide and heating the foamable composition sheet to crosslink, but a method of irradiating the foamable composition sheet with ionizing radiation to crosslink is preferred. It should be noted that the type and irradiation amount of ionizing radiation are as described in the first manufacturing method above.
[0169] Next, the foamable composition sheet can be foamed. When the foaming agent is a thermally decomposable foaming agent, the foamable composition sheet is heated to be foamed. The heating temperature and heating method are as described in the first manufacturing method mentioned above. In addition, the foamable composition sheet can be appropriately stretched while foaming or appropriately stretched after foaming. In this way, a foamed resin layer (foam) is obtained.
[0170] Then, the resin film or foamed body prepared separately for constituting the outer layer is superimposed and bonded with the foamed resin layer (foamed body), thereby the resin foam sheet can be obtained. Specifically, it can be heated and pressurized by a press machine, etc., and hot pressing is performed. Alternatively, it is also possible to apply an adhesive, an adhesive, etc. to the joint surface between the foamed resin layer and the outer layer, or to paste a double-sided adhesive tape, and to utilize an adhesive, an adhesive, a double-sided adhesive tape, etc. to bond.
[0171] (Third Manufacturing Method)
[0172] The multilayer resin foam sheet can also be manufactured by the following third manufacturing method. Specifically, it can be formed by pre-manufacturing a foamed body constituting the first resin layer, and applying a resin composition for forming the second resin layer on one or both sides of the foamed body (first resin layer). The third manufacturing method is suitable for the situation that the second resin layer is formed by a curable resin. For example, in the case of an acrylic resin, a resin composition comprising a monomer component (a) and a crosslinking agent, or a partially cured product of the resin composition, etc. can be applied to the first resin layer, and then cured, etc. to form the second resin layer.
[0173] The method for obtaining a resin foam sheet as a multi-layer laminate has been described as above, but in the case of obtaining a resin foam sheet consisting only of a foamed resin layer, the foamable composition sheet described in the above-mentioned second manufacturing method can be obtained, and the foamed resin layer (foam) can be obtained in the same manner as the above-mentioned second manufacturing method.
[0174] In the above description, the resin foam sheet of the present invention is described on the premise that bubbles are formed by a foaming agent, but bubbles do not necessarily need to be formed by a foaming agent. For example, the resin foam sheet can also be made by containing hollow particles inside.
[0175] [Adhesive tape]
[0176] The resin foam sheet of the present invention is preferably used as an adhesive tape substrate. The adhesive tape comprises the resin foam sheet of the present invention and an adhesive material disposed on at least one surface of the resin foam sheet. The adhesive tape can be bonded to other components through the adhesive material. The adhesive tape may be an adhesive tape with adhesive materials disposed on both sides of the resin foam sheet, or an adhesive tape with adhesive materials disposed on one side, preferably a double-sided adhesive tape with adhesive materials on both sides.
[0177] The adhesive material is a layer with pressure-sensitive adhesiveness, as long as it has at least an adhesive layer, and can be an adhesive layer monomer laminated on the surface of the resin foam sheet, or a double-sided adhesive sheet attached to the surface of the resin foam sheet, preferably an adhesive layer monomer. It should be noted that the double-sided adhesive sheet has a substrate and an adhesive layer arranged on both sides of the substrate. The double-sided adhesive sheet constituting the adhesive material is used to bond one adhesive layer to the resin foam sheet and to bond the other adhesive layer to other components.
[0178] In addition, you may further stick a release sheet, such as a release paper, on the adhesive material.
[0179] The thickness of the adhesive material is preferably 5 to 200 μm, more preferably 7 to 150 μm, and even more preferably 10 to 100 μm.
[0180] As the adhesive constituting the adhesive layer, for example, an acrylic adhesive, a polyurethane adhesive, a rubber adhesive, a silicone adhesive, etc. can be used, and among them, a silicone adhesive is preferred.
[0181] When using a silicone adhesive, it is usually difficult to achieve excellent adhesion to a tape substrate formed by a resin foam sheet. However, in the present invention, as described above, by using a resin foam sheet having a specific contact angle, the adhesion of the tape substrate (the resin foam sheet of the present invention) to the silicone adhesive can also be achieved to be excellent.
[0182] When the adhesive tape is a double-sided adhesive tape, any one of the adhesive materials provided on both sides of the tape substrate may have an adhesive layer formed of a silicone adhesive, but preferably both adhesive materials have an adhesive layer formed of a silicone adhesive.
[0183] When a double-sided adhesive sheet is used as the adhesive material, the adhesive layer bonded to the resin foam sheet of the two adhesive layers in the double-sided adhesive sheet constituting the adhesive material may be formed of a silicone adhesive, but preferably both adhesive layers use a silicone adhesive.
[0184] The resin foam sheet of the present invention is preferably used as a substrate for adhesive tape for fixing a wall hanging. Here, the wall hanging is a member for hanging various articles, and Figure 2 As shown, the wall hanging part can be a wall hanging part 20 including a base 21 and a hanging part 22 protruding from the base 21. The hanging part 22 can be in any shape, such as a hook, a rod, a hemisphere, a cube, a cuboid, a cone, etc. The base 21 is a component used to be fixed on the wall surface 25, such as Figure 2 As shown, the base 21 can be fixed to the wall surface 25 by the double-sided adhesive tape 15. Therefore, the base 21 can have a flat surface portion 21A for adhering the double-sided adhesive tape 15. The double-sided adhesive tape 15 includes an adhesive tape substrate 10 and adhesive materials 16A and 16B provided on both sides of the substrate 10. The adhesive tape substrate 10 can use the resin foam sheet of the present invention.
[0185] Of course, the resin foam sheet of the present invention can be used for purposes other than fixing wall hangings, can be used as a pressure-sensitive adhesive tape substrate for any purpose, and can be used for purposes other than a pressure-sensitive adhesive tape substrate.
[0186] Example
[0187] Hereinafter, the present invention will be described by way of examples, but the present invention is not limited to these examples. It should be noted that the methods for measuring the physical properties and the methods for evaluating the resin foam sheet are as follows.
[0188] <Thickness of Foamed Resin Layer and Outer Layer>
[0189] A cross section of the resin foam sheet was photographed using a digital microscope (manufactured by Keyence Co., Ltd., product name VHX-900), and the thickness of the middle layer (first resin layer) and each outer layer (second resin layer) was measured from the photographed image. In addition, the total thickness of the middle layer and the two outer layers was taken as the total thickness of the resin foam sheet.
[0190] <Apparent density and expansion ratio>
[0191] The apparent density of the resin foam sheets, first resin layer (middle layer) and second resin layer (outer layer) obtained in Examples and Comparative Examples was measured according to JIS K 7222, and the reciprocal thereof was taken as the expansion ratio. In Table 1, the expansion ratio of the resin foam sheet is described as the total expansion ratio.
[0192] <Closed Porosity>
[0193] A flat square test piece with a side length of 5 cm was cut from the resin foam sheet of the embodiment and the comparative example. Then, the thickness of the test piece was measured, the apparent volume V1 of the test piece was calculated, and the mass W1 of the test piece was measured. Next, the volume V2 occupied by the bubbles was calculated based on the following formula. It should be noted that the density of the test piece is designated as ρ (g / cm 3 ).
[0194] The volume occupied by the bubble V2 = V1-W1 / ρ
[0195] Next, the test piece was immersed in 23°C distilled water at a depth of 100 mm from the water surface, and a pressure of 15 kPa was applied to the test piece for 3 minutes. Then, the test piece was taken out of the water, the water attached to the surface of the test piece was removed, the mass W2 of the test piece was measured, and the closed porosity F1 was calculated based on the following formula.
[0196] Closed-cell rate F1 (%) = 100-100 × (W2-W1) / V2
[0197] <25% compression strength>
[0198] The 25% compressive strength of the resin foam sheets obtained in Examples and Comparative Examples was measured in accordance with JIS K6767.
[0199] <Oxygen Atom Content>
[0200] The element distribution on the surface of the resin foam sheet was analyzed using an energy dispersive X-ray analyzer in a scanning electron microscope ("JSM-IT100" manufactured by JEOL Ltd.), and the oxygen atom content (mass %) was measured.
[0201] <Contact angle>
[0202] The contact angle of the surface of the resin foam sheet was measured using "DM-701" manufactured by KYOWA Co., Ltd. in accordance with JIS K 6768. 5 mL of pure water (wetting tension 73 mN / m) was dropped onto the smooth surface and the measurement was performed after stabilization.
[0203] <Suspension test>
[0204] like Figure 3 As shown, first, a resin foam sheet 10 (size 100 mm×100 mm) is pasted to the wall surface 25 via an adhesive tape 30. Here, the shear adhesion of the adhesive tape 30 is sufficiently higher than that of the silicone double-sided adhesive tape 31 described later. In this hanging test, when the wall hanging 20 is peeled off, peeling occurs at the interface between the resin foam sheet 10 and the silicone double-sided adhesive tape 31. Next, the wall hanging 20 having a hook as a hanging portion 22 is pressed onto the resin foam sheet 10 via the silicone double-sided adhesive tape 31 under a load of 1 kg and 5 seconds, thereby pasting the wall hanging 20 to the resin foam sheet 10. Then, a weight 32 of 1.1 kg is hung on the hook of the wall hanging 20 and left to stand, and the time until the wall hanging 20 is peeled off from the resin foam sheet 10 is measured as the holding time. The test is carried out at room temperature (23°C).
[0205] It should be noted that the wall hanging fixture 20 and the silicone double-sided adhesive tape 31 are made of the product name "Comand TMThe commercially available product is "Fuck Outdoor CMO-30" (manufactured by 3M Co.). The silicone double-sided adhesive tape 31 has adhesive layers formed of a silicone adhesive on both sides of a substrate.
[0206] <Example 1>
[0207] As the polyolefin resin for the middle layer, a linear low-density polyethylene resin obtained using a metallocene catalyst (manufactured by Japan Polyethylene Co., Ltd., trade name "Kanel KF283", density: 0.921 g / cm 3 ), azodicarbonamide as a thermal decomposition type foaming agent. In addition, zinc oxide (manufactured by Sakai Chemical Industry Co., Ltd., trade name "OW-212F") as a decomposition temperature regulator and 2,6-di-tert-butyl-p-cresol as an antioxidant and belonging to a phenolic antioxidant are prepared. 100 parts by mass of a polyolefin resin, 8.0 parts by mass of a thermal decomposition type foaming agent, 1 part by mass of a decomposition temperature regulator, and 0.5 parts by mass of an antioxidant are supplied to the second extruder, respectively, and melt-kneaded at 130°C to prepare a foamable composition for the middle layer. Next, an ethylene-vinyl acetate copolymer (manufactured by Tosoh Corporation, trade name "ウルトラセン (registered trademark) 626") is prepared as a raw material for the outer layer resin composition. 100 parts by mass of an ethylene-vinyl acetate copolymer and 0.5 parts by mass of an antioxidant are supplied to the first extruder and the third extruder, respectively, and melt-kneaded at 130°C to prepare a resin composition for the outer layer.
[0208] The foamable composition for the middle layer is co-extruded from the second extruder, and the resin composition for the outer layer is co-extruded from the first extruder and the third extruder, thereby obtaining an unfoamed multilayer sheet having a layer formed of the foamable composition for the outer layer and layers formed of the resin composition for the outer layer laminated on both sides of the layer.
[0209] Next, the multilayer sheet is irradiated with 2.5 Mrad of electron beam at an acceleration voltage of 500 kV for cross-linking, and then continuously fed into a foaming furnace maintained at 250°C using hot air and infrared heaters for heating and foaming, thereby obtaining a resin foam sheet having a three-layer structure of an outer layer (resin film layer), a middle layer (foamed resin layer) and an outer layer (resin film layer) in sequence.
[0210] <Example 2>
[0211] A resin foam sheet was prepared in the same manner as in Example 1 except that the raw material of the outer layer resin composition was changed to an acid-modified polyolefin resin (Tokyo Material Co., Ltd., trade name "BONDINE TX8030", maleic anhydride-modified polyethylene resin, acid modification amount 3 mass %).
[0212] <Example 3>
[0213] A resin foam sheet was prepared in the same manner as in Example 1 except that the raw material of the outer layer resin composition was changed to an acid-modified polyolefin resin (Tokyo Material Co., Ltd., trade name "OREVAC 18362", maleic anhydride-modified polyethylene resin, acid modification amount 0.1 mass %).
[0214] <Example 4>
[0215] A resin foam sheet was prepared in the same manner as in Example 1 except that the raw material of the outer layer resin composition was changed to an olefin copolymer resin (manufactured by Sumitomo Chemical Co., Ltd., trade name "Acryfute WH206", ethylene-methyl methacrylate copolymer).
[0216] <Example 5>
[0217] A resin foam sheet having a three-layer structure of an outer layer (foamed resin layer), a middle layer (foamed resin layer) and an outer layer (foamed resin layer) was obtained in the same manner as in Example 1 except that 1.0 part by mass of a thermally decomposable foaming agent and 1 part by mass of a decomposition temperature regulator were added to the raw materials of the outer layer resin composition.
[0218] <Example 6>
[0219] The raw material of the outer layer resin composition was changed to a mixture of a linear low-density polyethylene resin (trade name "カーネルKF283") and an acid-modified polyolefin resin (trade name "BONDINE TX8030") in a ratio of 8:2 (mass ratio), and the amount of the foaming agent was changed as shown in Table 1. A resin foam sheet was prepared by the same method as in Example 1.
[0220] <Example 7>
[0221] A resin foam sheet was prepared in the same manner as in Example 1 except that the raw material of the outer layer resin composition was changed to a mixture of a linear low-density polyethylene resin (trade name "Kanel KF283") and an acid-modified polyolefin resin (trade name "BONDINE TX8030") in a ratio of 65:35 (mass ratio).
[0222] <Example 8>
[0223] The raw material of the outer layer resin composition was changed to a mixture of 8:2 (mass ratio) of a linear low-density polyethylene resin (trade name "カーネルKF283") and an acid-modified polyolefin resin (Tokyo Material Co., Ltd., trade name "LOTADOR AX8900", epoxy-modified polyethylene resin, modification amount 8 mass %), and the amount of the foaming agent was changed as shown in Table 1. Except for this, a resin foam sheet was prepared using the same method as Example 1.
[0224] <Examples 9 and 10>
[0225] The same operation as in Example 8 was carried out except that the blending amount of the thermally decomposable foaming agent in the middle layer resin layer composition was changed as shown in Table 1.
[0226] <Example 11>
[0227] A resin foam sheet was prepared by the same method as in Example 1, except that the raw material of the resin composition for the outer layer was changed to a mixture of 8:2 (mass ratio) of a linear low-density polyethylene resin (trade name "カーネルKF283") and an acid-modified polyolefin resin (manufactured by SK Polymer Co., Ltd., trade name "Primacor 3440", an acrylic acid-modified polyethylene resin, acid modification amount 9 mass %).
[0228] <Comparative Example 1>
[0229] A resin foam sheet was prepared in the same manner as in Example 1 except that the raw material of the resin composition for the outer layer was changed to a linear low-density polyethylene resin (manufactured by Japan Polyethylene Co., Ltd., trade name "Kanel KF283").
[0230] <Comparative Example 2>
[0231] A resin foam sheet was produced in the same manner as in Example 1 except that the outer layer was removed.
[0232] <Comparative Example 3>
[0233] 75 parts by mass of methyl acrylate (manufactured by Nippon Shokubai Co., Ltd.), 25 parts by mass of butyl acrylate (manufactured by Nippon Shokubai Co., Ltd.), and 0.5 parts by mass of a photopolymerization initiator (manufactured by BASF Japan Co., Ltd., trade name "Irgacure 184") were mixed and partially polymerized by ultraviolet polymerization to adjust the viscosity of the syrupy curable acrylic resin composition to 2000 mPa·s. 2 parts by mass of a bifunctional crosslinking agent (trade name "NKESTER APG-400", manufactured by Shin-Nakamura Chemical Co., Ltd.), 1 part by mass of a trifunctional crosslinking agent (trade name "NK ESTER A-9300-3CL", manufactured by Shin-Nakamura Chemical Co., Ltd.), and 2 parts by mass of hollow particles (trade name "Expancel 920DE80d30", manufactured by Nippon Phylight Co., Ltd.) were added to the resin composition and mixed to prepare a final curable acrylic resin composition. The obtained product was coated on a release paper at 23°C and irradiated with ultraviolet light to prepare a resin foam sheet with a thickness of 200 μm. It should be noted that the ultraviolet light was irradiated at an illumination of 4 mW / cm 2 , Light intensity: 720mJ / cm 2 irradiation under the conditions of .
[0234] <Comparative Examples 4 and 5>
[0235] The same operation as in Comparative Example 1 was carried out except that the blending amount of the thermally decomposable foaming agent in the middle layer resin layer composition was changed as shown in Table 1.
[0236]
[0237] A※3 hours↑ in the hanging test means that even after 3 hours, the wall hanging parts did not peel off, and the holding time was more than 5 minutes.
[0238] As shown in Table 1 above, in each embodiment, since a resin foam sheet having a first resin layer and a second resin layer, a contact angle of 36 to 95°, and a 25% compression strength of 250 kPa or less is used, the flexibility is high and the shear holding force can be improved. Therefore, as shown in the hanging test, even if the resin foam sheet is used for the adhesive tape for fixing wall hangings whose adhesive is a silicone adhesive, it is possible to prevent the wall hangings from falling.
[0239] In contrast, in Comparative Examples 1, 2, 4, and 5, since a resin foam sheet having a contact angle greater than 95° was used as the resin foam sheet, the shear holding force could not be improved, and if used in an adhesive tape for fixing a wall hanging part whose adhesive was a silicone adhesive, the wall hanging part would fall off in a short time. In addition, in Comparative Example 3, since a resin foam sheet having a compression strength greater than 250 kPa was used as the resin foam sheet, the softness of the resin foam sheet could not be ensured.
[0240] Explanation of symbols
[0241] 10. Resin foam sheet (tape base material)
[0242] 11. First resin layer (middle layer)
[0243] 12A, 12B second resin layer (outer layer)
[0244] 15 Double-sided adhesive tape
[0245] 16A, 16B bonding material
[0246] 20 Wall Mounts
[0247] 21 base
[0248] 22 Suspension
[0249] 25 wall
[0250] 30 Adhesive tape
[0251] 31. Silicone double-sided adhesive tape
[0252] 32 weights
Claims
1. A resin foam sheet comprising a first resin layer as a foamed resin layer, and a second resin layer which is provided on at least one surface of the first resin layer and is either a foamed resin layer or a resin film layer, wherein the contact angle of at least one surface is 36 to 95°, and the 25% compressive strength is 250 kPa or less. 2 . The resin foam sheet according to claim 1 , wherein the thickness of the resin foam sheet is 0.1 to 3.0 mm.
3. The resin foam sheet according to claim 1, wherein the foaming ratio of the resin foam sheet is 1.5 to 20 cm 3 / g. The resin foam sheet according to claim 1 , which has a closed-cell structure. The resin foam sheet according to any one of claims 1 to 4, comprising a middle layer composed of the first resin layer, and outer layers, namely, second resin layers, provided on both surfaces of the middle layer and composed of either a foamed resin layer or a resin film layer.
6. The resin foam sheet according to claim 5, wherein the foaming ratio of the outer layer is 1 to 3 cm 3 / g, and the foaming ratio of the middle layer is 3 to 20 cm 3 / g. 7 . The resin foam sheet according to claim 5 , wherein the middle layer comprises a polyolefin resin, and the outer layer comprises at least one selected from the group consisting of a polyolefin resin, a modified polyolefin resin, and an acrylic resin. The resin foam sheet according to claim 5 , wherein the outer layers are all resin film layers. 9 . The resin foam sheet according to claim 5 , wherein the oxygen atom content of the two outer layers is 3.5% by mass or more.
10. The resin foam sheet according to claim 1, which is used as a substrate of an adhesive tape for fixing a wall hanging.
11. The resin foam sheet according to claim 1, wherein the holding time in the following hanging test is 5 minutes or more; <Suspension test> A wall hanging part having a hook is pressed onto a resin foam sheet attached to the wall surface through a silicone double-sided adhesive tape under the conditions of a load of 1 kg and 5 seconds, thereby attaching the wall hanging part to the resin foam sheet; then, a 1.1 kg weight is hung on the hook of the wall hanging part and allowed to stand, and the time until the wall hanging part peels off the resin foam sheet is measured as the holding time. 12 . An adhesive tape comprising the resin foam sheet according to claim 1 and an adhesive material located on at least one surface of the resin foam sheet.