Method for preparing metal organic framework by microwave-assisted synthesis and metal organic framework prepared thereby

The preparation process of metal organic framework for polyethylene terephthalate plastic waste is simplified through microwave-assisted synthesis method, solving the problems of complex steps and high energy in the existing technology, and achieving efficient and simple metal organic framework production. Maintain product quality.

CN119032128APending Publication Date: 2024-11-26PTT EXPLORATION & PROD PUBLIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380020697.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-28
Filing Date
2023-01-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art In the preparation of polyethylene terephthalate plastic waste for metal organic framework synthesis, the steps are complex and energy-consuming, and the purification steps of terephthalic acid are required to affect efficiency and environmental impact.

Method used

The metal precursor was reacted with the polyethylene terephthalate plastic mixture by microwave-assisted synthesis method, simplifying the steps and preparing the metal organic framework without the need for purification of terephthalic acid.

Benefits of technology

The preparation of metal organic skeletons with simple steps, energy saving and time-reduced is achieved, and the product quality is similar to that of traditional methods, which can significantly reduce processing time and improve yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004982405050000071
    Figure BDA0004982405050000071
  • Figure BDA0004982405050000081
    Figure BDA0004982405050000081
  • Figure BDA0004982405050000082
    Figure BDA0004982405050000082
Patent Text Reader

Abstract

The invention relates to a method for preparing a metal organic framework. The method comprises the step that a mixture containing a metal precursor and polyethylene glycol terephthalate plastic is reacted through microwave-assisted synthesis. The invention also relates to the metal organic framework prepared by the method. According to the method for preparing the metal organic framework, disclosed by the invention, the polyethylene glycol terephthalate plastic waste can be utilized, so that environmental problems can be favorably reduced. In addition, the method can be conveniently executed, tedious and complex steps are not needed, and energy is saved in the preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The chemistry relates to a method for preparing a metal organic framework using microwave assisted synthesis and the metal organic framework prepared thereby. Background Art

[0002] Plastic is a synthetic material that plays an important role in everyday life and is increasingly used due to its desirable properties, low price, and high plasticity. As a result, plastic products are currently widely used, resulting in an increase in plastic waste every year. Some plastic waste is not a self-degradable material or takes hundreds of years to degrade, causing environmental impacts and plastic waste management issues.

[0003] Polyethylene terephthalate (PET) is one of the plastics commonly used to make products such as beverage bottles, packaging boxes or packaging bags because of its light weight, transparent, sticky properties and good impact resistance. However, most of the PET plastic waste currently generated is usually buried in landfills or burned in incinerators. Only a small amount is recycled because the recycling process is complicated and includes many steps, from sorting the product ingredients by plastic type, cleaning, chemical treatment to degrade the chemical components to forming new products. All these steps not only consume a lot of energy, but also may release harmful chemicals into the environment. Therefore, people try to find a way to increase the value of PET plastic waste and maximize its utilization to reduce the impact on the environment.

[0004] One approach currently being investigated to utilize polyethylene terephthalate plastic waste is to use it in metal-organic framework synthesis, since polyethylene terephthalate consists of a major component that can be converted into terephthalic acid (BDC), which can be used as a source of organic linkers in metal-organic framework synthesis.

[0005] The following patent documents disclose examples of prior art related to the use of polyethylene terephthalate plastic waste in metal organic framework synthesis.

[0006] Chinese patent publication number CN110283353A discloses a method for preparing a metal organic framework by using polyacid to degrade polyester plastic waste (such as PET). The method comprises the following steps: adding a polyacid precursor to a sodium acetate buffer solution, mixing until clear, adding polyester plastic waste fragments, mixing at a temperature of 170°C to 190°C for 60 to 80 hours, and then cooling, washing and drying to obtain a metal organic framework product.

[0007] Chinese patent publication number CN108676174A discloses a method for preparing a metal organic framework using polyethylene terephthalate plastic waste, comprising subjecting Zn(NO)3)2·6H2O and polyethylene terephthalate plastic waste to a solvothermal reaction at a temperature of 150°C for 24 hours, then washing the resulting reaction solution with N-methylpyrrolidone and methanol solution, and drying under vacuum.

[0008] U.S. Patent Publication No. US2021122898A1 discloses the preparation of metal organic frameworks from plastic waste using mechanochemical synthesis, wherein the preparation is carried out by grinding the reaction mixture by controlling relevant variables (such as impact force, grinding time, grinding ball size, temperature range and pressure, etc.).

[0009] However, in addition to the above-mentioned prior art, there is still a need to develop the application of polyethylene terephthalate plastic waste in the preparation of metal organic frameworks, and in particular, there is a need to develop a method for preparing metal organic frameworks from polyethylene terephthalate plastic, which can be conveniently carried out with simple steps and saves energy and time in the preparation. Summary of the invention

[0010] An object of the present invention is to provide a method for preparing a metal organic framework from polyethylene terephthalate plastic waste, which method can be conveniently carried out without cumbersome and complicated steps, and saves energy and time in the preparation. In particular, the present invention aims to develop a method for preparing a metal organic framework from polyethylene terephthalate plastic waste, which method does not require a purification step of separating terephthalic acid and terephthalic acid before carrying out the synthesis of the metal organic framework.

[0011] Another object of the present invention is to provide a method for preparing a metal organic framework from polyethylene terephthalate plastic waste, which can be easily carried out and significantly reduces the processing time compared to the commonly available method for preparing a metal organic framework from polyethylene terephthalate plastic waste.

[0012] In one aspect, the present invention relates to a method for preparing a metal organic framework comprising reacting a mixture comprising a metal precursor and polyethylene terephthalate plastic using microwave assisted synthesis.

[0013] In another aspect, the invention relates to a metal organic framework prepared by the method according to the invention.

[0014] The method for preparing a metal organic framework using microwave-assisted synthesis according to the present invention can be easily and conveniently performed, with simple steps, energy saving, and short processing time, while maintaining a high yield. In addition, the quality of the obtained metal organic framework product is similar to that of the metal organic framework prepared by the conventional preparation method using purified terephthalic acid as a metal organic framework synthesis reactant. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is a graph showing a powder X-ray diffraction (PXRD) pattern of a metal organic framework example prepared according to the method of the present invention and a PXRD pattern of UiO-66 according to theory in a database.

[0016] Figure 2 is a graph showing the N2 adsorption isotherm of an example of a metal organic framework prepared according to the method of the present invention.

[0017] Figure 3 is a graph showing thermogravimetric analysis (TGA) of examples of metal organic frameworks prepared from polyethylene terephthalate plastic samples obtained from 3 different sources. DETAILED DESCRIPTION

[0018] Unless otherwise stated, any aspect shown herein should also encompass application to other aspects of the invention.

[0019] Unless defined otherwise, technical and scientific terms used herein have the same meanings as understood by one of ordinary skill in the art.

[0020] In the present invention, the term "about" is used to indicate that any values ​​presented or shown herein may vary or deviate due to errors in the equipment or the methods used to determine the values.

[0021] The terms "consisting of," "comprising," "having," "containing," and "include" are open-ended verbs. For example, any method "consisting of," "comprising," "having," "containing," and "including" one or more components or one or more steps is not limited to only one component or one step or multiple steps or multiple components, but also covers unspecified components or steps.

[0022] Unless otherwise specified, the tools, equipment, methods, materials or chemicals mentioned herein refer to tools, equipment, methods, materials or chemicals commonly used or practiced by those skilled in the art.

[0023] All components and / or methods disclosed and claimed in the present invention are intended to cover aspects of the present invention obtained by actions, practices, modifications or changes of any factor, which do not require any experiments substantially different from the present invention, and according to the judgment of ordinary technicians in the field, give the same characteristics and utilities as the aspects of the present invention, and provide the same effects as the aspects of the present invention, even if there is no specific description in the claims. Therefore, substitutes or analogs of various aspects of the present invention and any slight modifications or changes that are obvious to ordinary technicians in the field are also considered to be within the spirit, scope and concept of the present invention.

[0024] The term "polyethylene terephthalate plastic" as used herein encompasses any plastic or copolymer with polyethylene terephthalate as a component, for example, polyethylene terephthalate plastics essentially comprise polyethylene terephthalate and may have additives as additional components. For example, polyethylene terephthalate plastics may comprise 80% to 100% by weight, or 85% to 100% by weight, or 85% to 95% by weight, or 80% to 95% by weight, or 80% to 90% by weight of polyethylene terephthalate compared to the gross weight of the polyethylene terephthalate plastic. Polyethylene terephthalate plastics according to the present invention may be obtained from different sources, for example, plastic bottles, plastic fibers, plastic sheets, plastic waste, plastic fragments in products, etc.

[0025] The above object of the present invention can be achieved by a method for preparing a metal organic framework having the following characteristics.

[0026] According to the present invention, a method for preparing a metal organic framework comprises reacting a mixture comprising a metal precursor and polyethylene terephthalate plastic using microwave assisted synthesis.

[0027] In a specific embodiment, the method for preparing a metal organic framework according to the present invention comprises the following steps:

[0028] (i) providing polyethylene terephthalate plastics with reduced size;

[0029] (ii) providing a mixture comprising a metal precursor and a polyethylene terephthalate plastic, the polyethylene terephthalate plastic being size-reduced in a solvent;

[0030] (iii) reacting the mixture of step (ii) using microwave assisted synthesis; and

[0031] (iv) isolating the reaction product obtained in step (iii), washing the reaction product with a solvent and drying it.

[0032] In an alternative embodiment, the method for preparing a metal organic framework according to the present invention may further comprise the step of microwave-assisted treatment of the size-reduced polyethylene terephthalate plastic under acidic, alkaline or neutral conditions before performing step (ii).

[0033] More specifically, the method for preparing a metal organic framework may further include a step of microwave-assisted heating of the size-reduced polyethylene terephthalate plastic at a temperature of 150° C. to 250° C. for 5 to 30 minutes before performing step (ii). Preferably, the step of microwave-assisted heating of the size-reduced polyethylene terephthalate plastic is performed under acidic conditions.

[0034] The method for preparing a metal organic framework according to the present invention is carried out so that all reactions are one-pot synthesis, without the need to separate and purify the terephthalic acid thus obtained before the microwave-assisted synthesis of the metal organic framework in step (iii).

[0035] According to the present invention, the particle size of the polyethylene terephthalate plastic reduced in size in step (i) is less than 1 cm, for example, the particle size is 0.01 cm to 1 cm or 0.05 cm to 1 cm, etc.

[0036] In another preferred aspect, the particle size of the polyethylene terephthalate plastic reduced in size in step (i) is less than 0.05 cm, for example, the particle size is 0.01 cm to 0.05 cm, etc.

[0037] The polyethylene terephthalate plastic is reduced in size by grinding, cutting, mechanochemical methods, shearing, tearing, or a combination thereof.

[0038] According to the present invention, the method for preparing a metal organic framework can be achieved by reacting a mixture containing a metal precursor and a polyethylene terephthalate plastic using microwave assisted synthesis. Preferably, the weight ratio of the metal precursor to the polyethylene terephthalate plastic in the mixture is 0.2:1 to 0.6:1.

[0039] In another preferred embodiment, the mixture further comprises an acid. Specifically, the mixture in step (ii) comprises a metal precursor, a size-reduced polyethylene terephthalate plastic and an acid.

[0040] Preferably, the weight ratio of the metal precursor to the acid in the mixture is 0.01:1 to 0.03:1.

[0041] More preferably, the weight ratio of polyethylene terephthalate plastic to acid in the mixture is from 0.02:1 to 0.07:1.

[0042] Examples of the acid used in the present invention are nitric acid, hydrochloric acid, sulfuric acid and mixtures thereof, with nitric acid being preferred.

[0043] According to the present invention, the metal precursor may be selected from the group consisting of zirconium (IV) salts, chromium (III) salts, iron (III) salts and mixtures thereof. Preferably, the metal precursor is a zirconium (IV) salt.

[0044] The zirconium (IV) salt may be selected from the group consisting of zirconium tetrachloride (ZrCl4), zirconium oxychloride (ZrOCl2), zirconium oxychloride octahydrate (ZrOCl2.8H2O), zirconium acrylate (Zr(CH2CHCO2)4) and mixtures thereof.

[0045] According to the present invention, the method for preparing a metal organic framework can be achieved by performing microwave-assisted synthesis using a microwave frequency of not less than 2450 MHz.

[0046] Specifically, the microwave-assisted synthesis is carried out by heating the mixture at a temperature of 80° C. to 160° C. using a power of 100 to 400 watts for 10 to 240 minutes. Preferably, the microwave-assisted synthesis is carried out by heating the mixture at a temperature of 100° C. to 140° C. using a power of 100 to 400 watts for 30 to 90 minutes, more preferably 45 to 60 minutes.

[0047] As an example, a solvent selected from the group consisting of dimethylformamide, diethylformamide, water, dimethyl sulfoxide, and a mixture thereof may be used to carry out step (ii).

[0048] Furthermore, a solvent selected from the group consisting of acetone, ethyl acetate, methanol, ethanol, and a mixture thereof may be used to perform the washing in step (iv).

[0049] The separation of the reaction product in step (iv) may be performed by filtration or centrifugation; and the drying in step (iv) may be performed at a temperature of 80° C. to 160° C. Preferably, the drying is performed under vacuum.

[0050] In a specific embodiment, the polyethylene terephthalate plastic contains an additive. The additive can be selected from the group consisting of dipentyl phthalate (DPP), di(2-ethylhexyl) adipate (DEHA), dioctyl adipate (DOA), diisobutyl phthalate (DEP) and mixtures thereof.

[0051] In a specific embodiment, the polyethylene terephthalate plastic comprises 80% to 100% polyethylene terephthalate by weight of the polyethylene terephthalate plastic.

[0052] The metal organic framework prepared by the method according to the present invention can be used as a heavy metal pollutant adsorbent, for example, it can be used to adsorb arsenic, mercury or palladium.

[0053] Example

[0054] Now, the present invention will be described in more detail with reference to experimental examples and the accompanying drawings. However, these examples are not intended to limit the scope of the present invention.

[0055] 1. Methods for preparing metal organic frameworks

[0056] According to an embodiment of the metal organic framework of the present invention, which is a UiO-66 material prepared from used polyethylene terephthalate plastic bottles and zirconium salts, the preferred conditions were determined as follows.

[0057] 1) Used polyethylene terephthalate plastic bottles were cut into small pieces of about 0.5 cm to 0.7 cm, and then powdered into particles with a size of less than 425 μm to obtain powdered polyethylene terephthalate plastic samples.

[0058] 2) A specified amount of nitric acid (HNO3) was added to the powdered polyethylene terephthalate plastic sample and incubated in a container (EasyPrep Plus container) for 5 minutes to 30 minutes.

[0059] 3) The mixture obtained in 2) was subjected to microwave irradiation at a temperature of 150° C. (power of 100 W to 400 W) for 5 minutes.

[0060] 4) Add designated amounts of solvent (DMF) and zirconium salt.

[0061] 5) The mixture obtained in 4) was subjected to ultrasonic treatment for 10 minutes and then subjected to microwave irradiation (power of 100 W to 400 W) at a specified temperature and for a specified time.

[0062] 6) The obtained metal organic framework was separated by centrifugation and washed with solvents DMF and methanol, respectively.

[0063] 7) Drying the obtained metal organic framework product at 80° C. for 12 hours.

[0064] Further, using powder X-ray diffraction (PXRD) technology (results such as Figure 1 ), BET surface area and pore volume, and N2 adsorption isotherms (results as shown in Figure 2 as shown) and thermogravimetric analysis (TGA) (results as shown Figure 3 Analyze the prepared metal organic framework product example).

[0065] 2. Study on the optimal conditions for the preparation of metal organic frameworks

[0066] In the present invention, experiments were conducted to study the effects of acid content, temperature and time in microwave-assisted synthesis on the synthesized metal organic framework products, as described below.

[0067] 1) Study on the influence of acid content

[0068] The experiment was conducted by preparing a metal organic framework according to the above method using a weight ratio of polyethylene terephthalate plastic (hereinafter referred to as "PET") to nitric acid (HNO3) of about 0.02:1, 0.04:1 and 0.07:1 and a weight ratio of zirconium tetrachloride (ZrCl4) to nitric acid of about 0.01:1 (HNO3 10ml and 15ml) and 0.03:1 (HNO3 5ml). The experimental results are shown in Figure 2. Figure 1 And as shown in Table 1.

[0069] Table 1

[0070]

[0071]

[0072] Note:

[0073] a - treating the polyethylene terephthalate plastic with an acid using microwaves at 150°C for 5 minutes prior to adding the ZrCl4; and

[0074] - Microwave-assisted synthesis of metal-organic frameworks was carried out at 120 °C for 120 min;

[0075] b The concentration of HNO3 is 65% and the density is 1.39 g / ml.

[0076] c The yield was calculated compared to the initial zirconium amount.

[0077] Depend on Figure 1 It can be seen from the experimental results that the metal organic framework (Examples 1-3) prepared from the polyethylene terephthalate plastic sample using the method of the present invention has characteristics corresponding to and consistent with the theoretical PXRD spectrum of UiO-66 in the database.

[0078] In addition, it was found that increasing the weight ratio of polyethylene terephthalate plastic to acid from 0.02:1 (Example 3, HNO3 15ml) to 0.04:1 (Example 2, HNO3 10ml) and 0.07:1 (Example 1, HNO3 5ml), respectively, and increasing the weight ratio of zirconium tetrachloride to acid from 0.01:1 (Example 2, HNO3 10ml and Example 3, 15ml) to 0.03:1 (Example 1, HNO3 5ml) can improve the yield. When the weight ratio of polyethylene terephthalate plastic to nitric acid is 0.07:1 and the weight ratio of zirconium tetrachloride to nitric acid is 0.03:1 (Example 3), a yield of more than 70% and up to 84% can be achieved.

[0079] 2) Study on the influence of temperature and time in microwave-assisted synthesis

[0080] The experiment was conducted by preparing the metal organic framework according to the above method using a weight ratio of polyethylene terephthalate plastic to nitric acid of 0.04:1 and a weight ratio of zirconium tetrachloride to nitric acid of 0.01:1. Figure 1 And as shown in Table 2.

[0081] Table 2

[0082]

[0083]

[0084] Note:

[0085] a – Treating polyethylene terephthalate plastic with acid using microwaves at 150°C for 5 minutes before adding ZrCl4; and

[0086] - In the preparation of the examples, about 500 g of powdered polyethylene terephthalate plastic sample, about 200 g of zirconium tetrachloride and 10 ml of nitric acid were used.

[0087] b The yield in % was calculated compared to the initial amount of zirconium.

[0088] Figure 1 It is shown that the metal organic framework prepared from the polyethylene terephthalate plastic sample using the method of the present invention has features corresponding to and consistent with the theoretical PXRD pattern of UiO-66 in the database.

[0089] From the experimental results in Table 2, it is found that under the same synthesis time (120 minutes), increasing the temperature in the microwave-assisted synthesis step from 100°C to 120°C and 140°C, respectively, can slightly improve the yield, wherein a yield of more than 75% can be achieved (Example 2, Example 4 and Example 5).

[0090] At the same synthesis temperature (120°C), it was found that even with a synthesis time of only 30 minutes, a yield of up to 50% could be achieved. Increasing the synthesis time from 30 minutes to 60 minutes significantly increased the yield from 50% to 83%. However, increasing the synthesis time from 60 minutes to 90 minutes resulted in a decrease in the yield from 83% to 73%.

[0091] 3) Polyethylene terephthalate plastic example

[0092] The experiment was conducted by using three different sources of polyethylene terephthalate plastic bottle waste examples, with a weight ratio of polyethylene terephthalate plastic to nitric acid of 0.04:1 and a weight ratio of zirconium tetrachloride to nitric acid of 0.01:1, and preparing the metal organic framework according to the above method. The experimental results are shown in Figure 3 shown.

[0093] Figure 3 The graph shows the thermogravimetric analysis (TGA) of metal organic frameworks prepared from polyethylene terephthalate plastic waste from different sources. Figure 3 In the present invention, it was found that the metal organic framework products prepared by the method of the present invention using polyethylene terephthalate plastic samples from three sources showed degradation corresponding to weight loss % of 85.02% (source 1), 86.11% (source 2) and 86.38% (source 3), respectively, and incomplete decomposition of the remaining ash of 14.98% (source 1), 13.89% (source 2) and 13.62% (source 3). These experimental results show that the metal organic frameworks from three sources have similar thermal stability and purity. Therefore, the method for preparing a metal organic framework according to the present invention is an effective method because it can be applied to general polyethylene terephthalate plastic waste from any source.

[0094] All of the above experimental results indicate that the method for preparing a metal organic framework from polyethylene terephthalate plastic waste according to the present invention not only helps to reduce environmental problems, but also can shorten the synthesis time while maintaining a high yield %, compared with commonly available methods.

[0095] Best Mode of the Invention

[0096] The best mode of the present invention is as described in the detailed description of the present invention.

Claims

1. A method for preparing a metal organic framework, comprising reacting a mixture comprising a metal precursor and polyethylene terephthalate plastic using microwave assisted synthesis.

2. The method according to claim 1, comprising the steps of: (i) providing polyethylene terephthalate plastics with reduced size; (ii) providing a mixture comprising a metal precursor and a polyethylene terephthalate plastic, wherein the polyethylene terephthalate plastic is size-reduced in a solvent; (iii) reacting the mixture of step (ii) using microwave assisted synthesis; and (iv) isolating the reaction product obtained in step (iii), washing the reaction product with a solvent and drying it.

3. The method according to claim 2, further comprising the step of microwave assisted heating the size-reduced polyethylene terephthalate plastic at a temperature of 150°C to 250°C for 5 minutes to 30 minutes before performing step (ii).

4. The method according to claim 3, wherein: The step of microwave assisted heating of the size-reduced polyethylene terephthalate plastic is performed under acidic conditions.

5. The method according to any one of claims 2 to 4, wherein: The particle size of the size-reduced polyethylene terephthalate plastic is less than 1 cm.

6. The method according to claim 5, wherein: The size-reduced polyethylene terephthalate plastic has a particle size of less than 0.05 cm.

7. The method according to any one of claims 2 to 6, wherein: The polyethylene terephthalate plastic is reduced in size by grinding, cutting, mechanochemical methods, shearing, tearing, or a combination thereof.

8. The method according to claim 1 or 2, wherein: The weight ratio of the metal precursor to the polyethylene terephthalate plastic in the mixture is 0.2:1 to 0.6:

1.

9. The method according to claim 1 or 2, wherein: The mixture also includes an acid.

10. The method according to claim 9, wherein: The weight ratio of the metal precursor to the acid in the mixture is 0.01:1 to 0.03:

1.

11. The method according to claim 9, wherein: The weight ratio of polyethylene terephthalate plastic to acid in the mixture is 0.02:1 to 0.07:

1.

12. The method according to any one of claims 4 or 9 to 11, wherein The acid is nitric acid, hydrochloric acid, sulfuric acid or a mixture thereof.

13. The method according to any one of claims 1, 2, 8 or 10, wherein: The metal precursor is selected from the group consisting of zirconium (IV) salts, chromium (III) salts, iron (III) salts and mixtures thereof.

14. The method according to claim 13, wherein: The zirconium (IV) salt is selected from the group consisting of zirconium tetrachloride (ZrCl4), zirconium oxychloride (ZrOCl2), zirconium oxychloride octahydrate (ZrOCl2.8H2O), zirconium acrylate (Zr(CH2CHCO2)4) and mixtures thereof.

15. The method according to claim 1 or 2, wherein: The microwave-assisted synthesis is performed using a microwave frequency of not less than 2450 MHz.

16. The method according to any one of claims 1, 2 or 15, wherein: The microwave-assisted synthesis is performed by heating the mixture at a temperature of 80°C to 160°C using a power of 100 to 400 watts for 10 to 240 minutes.

17. The method according to claim 16, wherein: The microwave-assisted synthesis is performed by heating the mixture at a temperature of 100° C. to 140° C. using a power of 100 to 400 watts for 30 to 90 minutes.

18. The method according to claim 2, wherein: The solvent in step (ii) is selected from the group consisting of dimethylformamide, diethylformamide, water, dimethyl sulfoxide and mixtures thereof.

19. The method according to claim 2, wherein: The solvent in step (iv) is selected from the group consisting of acetone, ethyl acetate, methanol, ethanol and mixtures thereof.

20. The method according to claim 2, wherein: The separation of the reaction product in step (iv) is carried out by filtration or centrifugation.

21. The method according to claim 2, wherein: The drying in step (iv) is carried out at a temperature of 80°C to 160°C.

22. The method according to any one of claims 1 to 21, wherein: Polyethylene terephthalate plastic contains additives.

23. The method according to claim 22, wherein: The additive is selected from the group consisting of dipentyl phthalate (DPP), di(2-ethylhexyl) adipate (DEHA), dioctyl adipate (DOA), diisobutyl phthalate (DEP) and mixtures thereof.

24. The method according to any one of claims 1 to 8, 11 or 22, wherein: The polyethylene terephthalate plastic contains 80% to 100% by weight of polyethylene terephthalate of the polyethylene terephthalate plastic.

25. A metal organic framework prepared by the method according to any one of claims 1 to 24.

26. The metal organic framework according to claim 25, which is used as a heavy metal pollutant adsorbent.