Antifouling coating composition
By using antifouling coating compositions with curable organopolysiloxane and glycerol condensate esters, combined with inorganic fillers and silane coupling agents, the silicone-based antifouling coating is solved inadequate antifouling properties of aquatic biological secretions by silicone-based antifouling coatings. The problem of this has achieved efficient and safe anti-fouling effect.
Patent Information
- Application Number
- CN202380034500.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-22
- Filing Date
- 2023-04-18
- Publication Date
- 2024-11-26
AI Technical Summary
The existing silicone-based antifouling coatings are insufficient to the membrane antifouling properties of aquatic biological secretions, and traditional slip agents have insufficient safety and environmental responsiveness, resulting in low antifouling effect.
Antifouling coating compositions containing curable organopolysiloxane and specific glycerol condensate esters are used, combined with inorganic fillers and silane coupling agents to form high antifouling, safe and environmentally friendly antifouling coatings. membrane.
It achieves efficient anti-fouling properties for aquatic organisms, improves the anti-fouling performance and safety of the coating film, and is suitable for anti-fouling applications of ships and water structures.
Smart Images

Figure CN119032143A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an antifouling coating composition, an antifouling coating film, an antifouling sheet, a substrate with an antifouling coating film, a method for producing the same, and an antifouling method. Background Art
[0002] To prevent economic losses such as increased propulsion resistance and damage due to erosion caused by the attachment of aquatic organisms, underwater structures such as the bottom of ships are required to be antifouled by aquatic organisms. Currently, the most common method for this antifouling is to use an antifouling coating film formed by applying an antifouling coating composition.
[0003] Examples of antifouling coating compositions include silicone-based antifouling coatings, which utilize silicone rubber as the main film-forming component and exhibit antifouling properties such as low surface free energy and film elasticity. These coatings offer advantages in terms of safety and environmental compatibility.
[0004] Patent Document 1 discloses an underwater antifouling pipe having excellent antifouling properties and excellent damage resistance even under conditions of high biofouling load in water, an underwater cable, and a method for protecting an underwater cable using the aforementioned underwater antifouling pipe. The pipe comprises a base layer mainly made of silicone, and an antifouling layer on the base layer containing a cured silicone (A) and a lubricant (B), the antifouling layer being the outermost layer.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 2021-028166 Summary of the Invention
[0008] Problems to be solved by the invention
[0009] Silicone-based antifouling coatings tend to have insufficient antifouling properties, particularly against films secreted by aquatic organisms, such as slime. To compensate for this, as described in Patent Document 1, lubricants such as silicone oil and paraffin oil that ooze out onto the surface of the antifouling coating film at a moderate rate are sometimes incorporated.
[0010] However, in view of suitability for marine applications, agents with better safety and environmental compatibility than these lubricants are desired, but such materials generally have a problem of low antifouling effect.
[0011] The present invention aims to provide an antifouling coating composition that is excellent in safety and environmental resistance and exhibits high antifouling properties against aquatic organisms. Another object of the present invention is to provide an antifouling coating film, an antifouling sheet, an antifouling coating-coated substrate having the antifouling coating film, a method for producing the antifouling coating film, and an antifouling method using the antifouling coating film.
[0012] Means for solving problems
[0013] The present inventors have conducted intensive studies in view of the above-mentioned problems and have found that the above-mentioned problems can be solved by preparing an antifouling coating composition containing a curable organopolysiloxane (A) and a specific glycerin condensate ester (B), thereby completing the present invention.
[0014] The gist of the present invention is as follows.
[0015] The present invention relates to the following [1] to
[16] .
[0016] [1] An antifouling coating composition comprising a curable organopolysiloxane (A) and a glycerin condensate ester (B) represented by the following formula (1).
[0017] [Chemistry 1]
[0018]
[0019] (In the above formula (1), n is an integer of 2 or more and 20 or less, and R each independently represents a hydrogen atom or R 1 C(=O)-, at least one R is R 1 C(=O)-,R 1 represents a monovalent hydrocarbon group having 7 or more and 23 or less carbon atoms.
[0020] [2] The antifouling coating composition according to [1], wherein the R 1 Contains branched hydrocarbon groups.
[0021] [3] The antifouling coating composition according to [1] or [2], wherein the R contains an isostearyl group.
[0022] [4] The antifouling coating composition according to any one of [1] to [3], wherein at least one R is a hydrogen atom.
[0023] [5] The antifouling coating composition according to any one of [1] to [4], wherein the content of the glycerin condensate ester (B) in the solid content of the antifouling coating composition is 1% by mass or more and 20% by mass or less.
[0024] [6] The antifouling coating composition according to any one of [1] to [5], wherein the curable organopolysiloxane (A) is a compound represented by the following formula (A1).
[0025] [Chemistry 2]
[0026]
[0027] (In formula (A1), R 11 and R 13 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aralkyl group or a halogenated alkyl group having 1 to 16 carbon atoms, and R 12 Each independently represents a hydroxyl group or a hydrolyzable group, r represents an integer of 1 to 3, and p represents 10 to 10,000.
[0028] [7] The antifouling coating composition according to any one of [1] to [6], wherein the content of the curable organopolysiloxane (A) in the solid content of the antifouling coating composition is 50% by mass or more and 99% by mass or less.
[0029] [8] The antifouling coating composition according to any one of [1] to [7], further comprising an inorganic filler (C).
[0030] [9] The antifouling coating composition according to [8], wherein the inorganic filler (C) is silica, and the silica is incorporated into the antifouling coating composition in the form of a kneaded product with the curable organopolysiloxane (A).
[0031]
[10] The antifouling coating composition according to any one of [1] to [9], further comprising a silane coupling agent (D).
[0032]
[11] The antifouling coating composition according to any one of [1] to
[10] , further comprising one or more selected from silicone oil (E) and an acrylic polymer (F) having a hydrophilic group.
[0033]
[12] An antifouling coating film formed by curing the antifouling coating composition according to any one of [1] to
[11] .
[0034]
[13] An antifouling sheet having the antifouling coating film described in
[12] .
[0035]
[14] A substrate with an antifouling coating film, which has the antifouling coating film described in
[12] or the antifouling sheet described in
[13] on the substrate.
[0036]
[15] The substrate with an antifouling coating according to
[14] , wherein the substrate is selected from ships, underwater structures and fishery materials.
[0037]
[16] A method for producing a substrate with an antifouling coating film, the method comprising a step (1) of applying or impregnating the antifouling coating composition described in any one of [1] to
[11] onto a substrate to obtain a coating or impregnation product, and a step (2) of curing the coating or impregnation product.
[0038]
[17] An antifouling method using the antifouling coating film described in
[12] or the antifouling sheet described in
[13] .
[0039] Effects of the Invention
[0040] According to the present invention, an antifouling coating composition can be provided that is excellent in safety and environmental resistance and has high antifouling properties against aquatic organisms. Furthermore, according to the present invention, an antifouling coating film and an antifouling sheet using the antifouling coating composition can be provided, as well as a substrate with the antifouling coating film and a method for producing the same, and an antifouling method using the antifouling coating film. DETAILED DESCRIPTION
[0041] Hereinafter, the antifouling coating composition, the antifouling coating film, the antifouling sheet, the substrate with the antifouling coating film and the production method thereof, and the antifouling method according to the present embodiment will be described in detail.
[0042] [Antifouling coating composition]
[0043] The antifouling coating composition of the present embodiment (hereinafter also simply referred to as "coating composition") contains a curable organopolysiloxane (A) and a glycerin condensate ester (B) represented by the following formula (1).
[0044] [Chemistry 3]
[0045]
[0046] (In the above formula (1), n is an integer of 2 or more and 20 or less, and R each independently represents a hydrogen atom or R 1 C(=O)-, at least one R is R 1 C(=O)-,R 1 represents a monovalent hydrocarbon group having 7 or more and 23 or less carbon atoms.
[0047] The present invention provides an antifouling coating composition that is excellent in safety and environmental resistance and has high antifouling properties against aquatic organisms. Although the detailed reasons for the above effects are unknown, some of the reasons are considered as follows.
[0048] Since silicone-based antifouling coatings do not have coating film renewal properties, dissolution of the coating film into water is suppressed, resulting in excellent safety and environmental compatibility. Furthermore, it is believed that by containing a specific glycerol condensate ester (B) as a surface conditioner in the present invention, an antifouling coating film having excellent static and dynamic antifouling properties can be obtained using the antifouling coating composition of this embodiment.
[0049] Each component used in the antifouling coating composition will be described in detail.
[0050] <Curable organopolysiloxane (A)>
[0051] The coating composition of the present embodiment contains a curable organopolysiloxane for the purpose of improving the antifouling properties of the antifouling coating film.
[0052] The curable organopolysiloxane (A) used in this embodiment includes an organopolysiloxane having a main chain having a polyorganosiloxane structure and reactive groups. These reactive groups react with each other or with the reactive groups of the organosilicon crosslinking agent (H) described below to form a three-dimensional crosslinked structure and cure. Furthermore, the organopolysiloxane may react with a silane coupling agent described below.
[0053] Examples of the polyorganosiloxane structure include a polydimethylsiloxane structure and a polymethylphenylsiloxane structure. Among them, a polydimethylsiloxane structure is preferred. Alkylene groups, polyoxyalkylene groups, and the like may also exist in a block form.
[0054] Furthermore, as a linking site between the main chain and the reactive site, for example, an alkylene group, a polyoxyalkylene group, or the like may be present.
[0055] The reactive group is an addition reactive group or a condensation reactive group. In the curing reaction, the reactive group is preferably a condensation reactive group from the viewpoint of minimizing the influence of curing-inhibiting substances and obtaining a stable reaction rate.
[0056] Examples of the condensation-reactive group include silanol groups, oxime silyl groups, acyloxy silyl groups, alkoxy silyl groups, alkenyloxy silyl groups, amino silyl groups, and amido silyl groups. Preferred are silanol groups, oxime silyl groups, acyloxy silyl groups, alkoxy silyl groups, and alkenyloxy silyl groups. More preferred are silanol groups, oxime silyl groups, alkoxy silyl groups, and alkenyloxy silyl groups. Further preferred are silanol groups, oxime silyl groups, alkoxy silyl groups, and alkenyloxy silyl groups. Even more preferred are silanol groups, oxime silyl groups, alkoxy silyl groups, and alkenyloxy silyl groups. Further preferred are silanol groups and oxime silyl groups.
[0057] The oxime group is preferably an oxime group having 1 to 10 carbon atoms, more preferably dimethyl ketone oxime group, methyl ethyl ketone oxime group, diethyl ketone oxime group, methyl isopropyl ketone oxime group, and methyl isobutyl ketone oxime group, and still more preferably methyl ethyl ketone oxime group and methyl isobutyl ketone oxime group.
[0058] The alkoxy group is preferably an alkoxy group having 1 to 6 carbon atoms, preferably a methoxy group, an ethoxy group, a propoxy group, and a butoxy group, more preferably a methoxy group and an ethoxy group, and still more preferably a methoxy group.
[0059] Two or more oxime groups or alkoxy groups may be bonded to one silicon atom as the condensation-reactive group. Preferably, two or more oxime groups or alkoxy groups are bonded to one silicon atom.
[0060] Examples of the position of the reactive site include direct bonding to a silicon atom of the main chain, in a side chain, both ends of the main chain, and one end of the main chain. Both ends of the main chain are preferred.
[0061] The curable organopolysiloxane (A) is preferably a curable organopolysiloxane having a reactive group. Specific examples thereof include silicones containing silanol groups, silicones containing oximinosilyl groups, silicones containing alkoxy groups, and silicones containing enolsilyl ether groups. Silicones containing silanol groups, silicones containing oximinosilyl groups, and silicones containing alkoxy groups are preferred, and silicones containing silanol groups and silicones containing oximinosilyl groups are more preferred.
[0062] As the curable organopolysiloxane (A) having the reactive group, a compound that forms silicone rubber when cured is preferred, and for example, a compound represented by the following formula (A1) is preferred.
[0063] [Chemistry 4]
[0064]
[0065] (In formula (A1), R 11 and R 13 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aralkyl group or a halogenated alkyl group having 1 to 16 carbon atoms, and R 12 Each independently represents a hydroxyl group or a hydrolyzable group. In addition, r represents an integer of 1 to 3, and p represents 10 to 10000.
[0066] In formula (A1), R 11 and R 13 Each independently represents a hydrogen atom, an alkyl group having 1 to 16 carbon atoms, an alkenyl group, an aryl group, an aralkyl group, an alkoxy group or a halogenated alkyl group.
[0067] R 11 and R 13 The alkyl group in the group is an alkyl group having 1 to 16 carbon atoms, and examples thereof include methyl, ethyl, propyl, butyl, pentyl, hexyl, and heptyl.
[0068] R 11 and R 13The alkenyl group in is an alkenyl group having 2 to 16 carbon atoms, and examples thereof include vinyl, allyl, propenyl, isopropenyl, butenyl, isobutenyl, pentenyl, heptenyl, hexenyl, and cyclohexenyl.
[0069] R 11 and R 13 The aryl group in is an aryl group having 6 to 16 carbon atoms, and may have a substituent such as an alkyl group on the aromatic ring. Examples thereof include phenyl, tolyl (methylphenyl), xylyl (dimethylphenyl), and naphthyl.
[0070] R 11 and R 13 The aralkyl group in the group is an aralkyl group having 7 to 16 carbon atoms, and examples thereof include benzyl, 2-phenylethyl, 2-naphthylethyl, and diphenylmethyl.
[0071] R 11 and R 13 The haloalkyl group in the group is a haloalkyl group having 1 to 16 carbon atoms, and examples thereof include groups in which a part or all of the hydrogen atoms contained in the above-mentioned alkyl group are substituted with halogen atoms such as fluorine atoms, chlorine atoms, bromine atoms and iodine atoms.
[0072] Among them, R in formula (A1) 11 A hydrogen atom, an alkyl group, an alkenyl group, and an aryl group are preferred, a methyl group, an ethyl group, a vinyl group, and a phenyl group are more preferred, and a methyl group and a vinyl group are further preferred.
[0073] In addition, R in formula (A1) 13 A hydrogen atom, an alkyl group, an alkenyl group, and an aryl group are preferred, a methyl group, an ethyl group, a vinyl group, and a phenyl group are more preferred, a methyl group, an ethyl group, and a phenyl group are further preferred, and a methyl group and a phenyl group are further preferred.
[0074] It should be noted that there are multiple R 13 Each can be the same or different. 11 When there are multiple ones, they may be the same or different.
[0075] In formula (A1), R 12 Each independently represents a hydroxyl group or a hydrolyzable group.
[0076] As R 12 Examples of the hydrolyzable group include an oxime group, an acyloxy group, an alkoxy group, an alkenyloxy group, an amino group, an amide group, and an aminooxy group.
[0077] As R 12 The oxime group in the group preferably has a total carbon number of 1 to 10, and examples thereof include dimethyl ketone oxime, methyl ethyl ketone oxime, diethyl ketone oxime, methyl isopropyl ketone oxime, and methyl isobutyl ketone oxime.
[0078] As R 12 The acyloxy group (RC(=O)O-) in the group is preferably an aliphatic acyloxy group having 1 to 10 carbon atoms or an aromatic acyloxy group having 7 to 12 carbon atoms, and examples thereof include acetyloxy, propionyloxy, butyryloxy, and benzoyloxy.
[0079] As R 12 The alkoxy group in the alkoxy group is preferably an alkoxy group having a total carbon number of 1 to 10. 12 In the alkoxy group in , one or more oxygen atoms may be present between one or more carbon atoms.
[0080] As R 12 Specific examples of the alkoxy group in include methoxy, ethoxy, propoxy, butoxy, methoxyethoxy, and ethoxyethoxy.
[0081] As R 12 The alkenyloxy group in the group is preferably an alkenyloxy group having 3 to 10 carbon atoms, and examples thereof include isopropenyloxy, isobutenyloxy, and 1-ethyl-2-methylvinyloxy.
[0082] As R 12 The amino group in the group is preferably an amino group having 1 to 10 carbon atoms, and examples thereof include N-methylamino, N-ethylamino, N-propylamino, N-butylamino, N,N-dimethylamino, N,N-diethylamino, and cyclohexylamino.
[0083] As R 12 The amide group in the group is preferably an amide group having 2 to 10 carbon atoms in total, and examples thereof include N-methylacetamide, N-ethylacetamide, and N-methylbenzamide.
[0084] As R 12 The aminooxy group in the group preferably has 2 to 10 carbon atoms in total, and examples thereof include N,N-dimethylaminooxy and N,N-diethylaminooxy.
[0085] Among them, R in formula (A1) is excellent in curability and antifouling properties of the antifouling coating film formed. 12 A hydroxyl group, an oxime group, and an alkoxy group are preferred, a hydroxyl group and an oxime group are more preferred, and a hydroxyl group, a methyl ethyl ketoxime group, and a methyl isobutyl ketoxime group are further preferred.
[0086] When the antifouling coating film formed from the antifouling coating composition is a clear coating film not containing the pigment (J) as described below, a methyl isobutyl ketone oxime group is preferred from the viewpoint of achieving better transparency.
[0087] It should be noted that there are multiple R 12They can be the same or different.
[0088] In formula (A1), r represents an integer of 1 to 3.
[0089] In R 12 In the case of a hydroxyl group, r is preferably 1. 12 In the case of a substituent other than a hydroxyl group, r is preferably 2.
[0090] In formula (A1), p represents 10 to 10,000, preferably 100 to 1,000, and can be appropriately adjusted so as to satisfy the following weight average molecular weight.
[0091] It should be noted that p means -(SiR 13 2-O)-average number of repeats.
[0092] The weight average molecular weight (Mw) of the curable organopolysiloxane (A) is preferably 500 or more, more preferably 5000 or more, further preferably 10000 or more, further preferably 15000 or more, further preferably 20000 or more, and is preferably 1000000 or less, more preferably 100000 or less, further preferably 50000 or less, and further preferably 40000 or less, from the viewpoint of improving the workability during the production of the coating composition, the coating workability and curability of the coating composition, and the strength of the formed coating film.
[0093] In the present embodiment, the "weight average molecular weight (Mw)" and the "number average molecular weight (Mn)" described later are measured using GPC (gel permeation chromatography) and calculated by conversion using standard polystyrene having a known molecular weight.
[0094] In addition, the viscosity of the curable organopolysiloxane (A) at 25°C is preferably 20 mPa·s or more, more preferably 100 mPa·s or more, further preferably 500 mPa·s or more, further preferably 1000 mPa·s or more, and preferably 100,000 mPa·s or less, more preferably 10,000 mPa·s or less, further preferably 5,000 mPa·s or less, and further preferably 3,000 mPa·s or less, from the viewpoint of improving the workability during the production of the coating composition, improving the coating workability and curing properties of the coating composition, and improving the strength of the formed coating film.
[0095] In addition, the viscosity of the curable organopolysiloxane (A) at 25° C. in this specification is the viscosity measured by a B-type rotational viscometer (for example, Model BM, manufactured by Tokyo Keiki Co., Ltd.).
[0096] The content of the curable organopolysiloxane (A) in the coating composition is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less, from the viewpoint of improving the antifouling properties and strength of the antifouling coating film formed.
[0097] The content of the curable organopolysiloxane (A) in the solid content of the coating composition is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 65% by mass or more, and is preferably 99% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less.
[0098] It should be noted that the "solid content of the coating composition" in this specification refers to the components other than the organic solvent (K) described later and the volatile components contained as solvents in each component, and the "content in the solid content of the coating composition" can be calculated as the content in the solid content obtained by drying the coating composition in a hot air dryer at 125°C for 1 hour.
[0099] As the curable organopolysiloxane (A), a commercially available product can be used. Examples of commercially available products include "DMS-S35" manufactured by GELEST Co., Ltd. and "KE-445" manufactured by Shin-Etsu Chemical Co., Ltd. Alternatively, as the curable organopolysiloxane (A), compounds described in Japanese Patent Application Laid-Open No. 2001-139816 can be used.
[0100] <Glycerol Condensate Ester (B)>
[0101] The coating composition of this embodiment contains a glycerol condensate ester (B) represented by the following formula (1). By making the coating composition of this embodiment contain a specific glycerol condensate ester (B), it is possible to impart good slip properties to the antifouling coating film formed by the coating composition, thereby improving the adhesion barrier of aquatic organisms (antifouling properties).
[0102] [Chemistry 5]
[0103]
[0104] (In the above formula (1), n is an integer of 2 or more and 20 or less, and R each independently represents a hydrogen atom or R 1 C(=O)-, at least one R is R 1 C(=O)-,R 1 represents a monovalent hydrocarbon group having 7 or more and 23 or less carbon atoms.
[0105] In formula (1), with respect to n, from the viewpoints of antifouling property and availability, it is an integer of 2 or more and 20 or less, preferably an integer of 3 or more, more preferably an integer of 16 or less, still more preferably an integer of 12 or less, and further preferably an integer of 10 or less.
[0106] Each R independently represents a hydrogen atom or R 1 C(=O)-, and at least one R is R 1 C(=O)-, R 1 represents a monovalent hydrocarbon group having 7 or more and 23 or less carbon atoms. By making at least one R be R 1 C(=O)-, the coating workability, leveling property, appearance of the formed antifouling coating film, smoothness, and adhesion to the substrate and the undercoat coating film of the coating composition are excellent, and it is preferable in view of this.
[0107] Regarding the carbon number of R 1 from the viewpoint of antifouling property, it is preferably 9 or more, more preferably 11 or more, still more preferably 15 or more, and preferably 21 or less, more preferably 19 or less.
[0108] As the monovalent hydrocarbon group, it may be a saturated hydrocarbon group or an unsaturated hydrocarbon group. In addition, it may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. In addition, it may be linear, branched, or cyclic. As the monovalent hydrocarbon group, examples include an alkyl group, an alkenyl group, an aryl group, an aralkyl group, etc. Among them, R 1 preferably contains a branched hydrocarbon group, more preferably a branched hydrocarbon group, still more preferably a branched aliphatic hydrocarbon group, and further preferably a branched alkyl group.
[0109] R is preferably isostearoyl group, 2-ethylhexanoyl group, ricinoleoyl group (Japanese: リシノレイノイル基), and more preferably isostearoyl group.
[0110] The glycerol condensate ester (B) is a condensation ester compound of a fatty acid having 8 or more and 24 or less carbon atoms and polyglycerol.
[0111] Polyglycerol is a polymer obtained by condensing glycerol, and the glycerol condensate ester (B) is a compound obtained by mixing and heating a fatty acid having 8 or more and 24 or less carbon atoms and polyglycerol.
[0112] Examples of the fatty acid having 8 or more and 24 or less carbon atoms include octanoic acid, 2-ethylhexanoic acid, isononanoic acid, decanoic acid, lauric acid, palmitic acid, stearic acid, isostearic acid, behenic acid, oleic acid, erucic acid, hydroxystearic acid, ricinoleic acid, coconut oil fatty acid. Among them, isostearic acid, 2-ethylhexanoic acid, and ricinoleic acid are preferred, and isostearic acid is more preferred.
[0113] It should be noted that, in the glycerol condensate ester (B), from the perspective of coating workability of the coating composition, antifouling properties of the resulting antifouling coating film, and excellent adhesion to the substrate and primer coating film, at least one R is preferably a hydrogen atom. In other words, it is preferably not a completely esterified product, but rather at least a portion of the hydroxyl groups are present as is.
[0114] Glycerol condensate ester (B) has n+2 R. Among n+2 R, R is R 1 The ratio of C(=O)- is preferably 10% or more, more preferably 20% or more, further preferably 35% or more, further preferably 40% or more, and is preferably 95% or less, more preferably 90% or less, further preferably 85% or less.
[0115] The glycerol condensate ester (B) preferably has fluidity at 25°C, and is more preferably in a liquid state. It is believed that the fluidity of the glycerol condensate ester (B) improves its mobility within the antifouling coating film, thereby enhancing the effect of imparting slip to the surface. Furthermore, it is preferred because it reduces the viscosity of the coating composition, thereby improving coating properties.
[0116] As the glycerin condensate ester (B), commercially available products can be used, and examples thereof include the Elamex series (manufactured by Nippon Emulsion Co., Ltd.), the Nikkol series (manufactured by Nikko Chemical Co., Ltd.), the Sunsoft series, the Sun Oil series (manufactured by Taiyo Chemical Co., Ltd.), and the Sy Glyster / S Face series (manufactured by Sakamoto Pharmaceutical Industry Co., Ltd.). Among these, Elamex DISG-2, DISG-3, DISG-6, DISG-10, TISG-2, and TISG-10 are preferred in the Elamex series, NIKKOL Decaglyn 5-ISV and 10-ISV are preferred in the NIKKOL series, and S Face IS-1005P and IS-1009P are preferred in the Sy Glyster / S Face series.
[0117] The content of the glycerol condensate ester (B) in the coating composition is preferably 0.5% by mass or more, more preferably 1% by mass or more, further preferably 3% by mass or more, further preferably 4% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 12% by mass or less, further preferably 8% by mass or less, from the viewpoint of improving antifouling properties.
[0118] Furthermore, the content of the glycerol condensate ester (B) in the solid content of the coating composition is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, and is preferably 20% by mass or less, more preferably 17% by mass or less, even more preferably 15% by mass or less, and even more preferably 10% by mass or less, from the perspectives of coating workability and storage stability of the coating composition, and the antifouling properties of the antifouling coating film formed, adhesion to the substrate and the primer coating film, and excellent appearance.
[0119] The coating composition of this embodiment may contain other components in addition to the curable organopolysiloxane (A) and glycerol condensate ester (B). Examples of other components include an inorganic filler (C), a silane coupling agent (D), a silicone oil (E), an acrylic polymer having a hydrophilic group (F), an antifouling agent (G), an organosilicon crosslinking agent (H), a curing catalyst (I), a pigment (J), and an organic solvent (K).
[0120] Other components are described below in detail.
[0121] <Inorganic Filler (C)>
[0122] The coating composition of the present embodiment may contain an inorganic filler (C) for the purpose of improving the fluidity and thixotropy of the coating composition.
[0123] When the coating composition of this embodiment contains an inorganic filler (C), as described above, the fluidity and thixotropy of the coating composition are improved, and a sufficiently thick coating film can be formed even on vertical coating surfaces with a reduced number of coating applications. In addition, the physical properties of the resulting coating film, such as hardness, tensile strength, and elongation, are well-balanced and improved.
[0124] Examples of the inorganic filler (C) include silica, mica, calcium carbonate, aluminum carbonate, magnesium carbonate, barium carbonate, aluminum oxide, titanium oxide, aluminum hydroxide, aluminum silicate, magnesium silicate, potassium feldspar, zinc oxide, kaolin, alumina white, barium sulfate, calcium sulfate, zinc sulfide, and short glass fibers. These inorganic fillers may be used alone or in combination of two or more.
[0125] Among them, silica is preferred as the inorganic filler (C) from the viewpoint of improving the physical properties of the coating film, such as hardness, tensile strength, and elongation, in a well-balanced manner.
[0126] As silica, for example, hydrophilic silicas such as wet silica (hydrated silica), dry silica (fumed silica, anhydrous silica) (surface untreated silica) can be used. In addition, hydrophobic treated silica in which the surface of the above-mentioned silica has been hydrophobized can also be used, specifically hydrophobic wet silica, hydrophobic fumed silica, etc. These silicas can be used alone or in combination of two or more.
[0127] Among these, hydrophobic treated silica having its surface hydrophobized is preferred from the viewpoint of excellent dispersibility in the coating composition.
[0128] The wet-process silica is not particularly limited, but preferably has an adsorbed moisture content of 4 to 8% by mass, a bulk density of 200 to 300 g / L, a primary particle diameter of 10 to 30 μm, and a specific surface area (BET surface area) of 10 m 2 / g or more wet-process silica.
[0129] The dry-process silica is not particularly limited, but preferably has a water content of 1.5% by mass or less, a bulk density of 50 to 100 g / L, a primary particle diameter of 8 to 20 μm, and a specific surface area of 10 m 2 / g or more of dry-process silica.
[0130] Examples of the hydrophobic fumed silica include dry-process silica surface-treated with an organosilicon compound such as methyltrichlorosilane, dimethyldichlorosilane, hexamethyldisilazane, hexamethylcyclotrisiloxane, and octamethylcyclotetrasiloxane. The hydrophobic fumed silica has low water absorption over time, with a water content preferably being 0.3% by mass or less, and more preferably 0.1 to 0.2% by mass.
[0131] The hydrophobic fumed silica is not particularly limited, but preferably has a primary particle diameter of 5 to 50 nm, a bulk density of 50 to 100 g / L, and a specific surface area of 10 m 2 / g or more hydrophobic fumed silica. It should be noted that when the hydrophobic fumed silica is subjected to a heat treatment described below, the amount of water adsorbed on the surface of the hydrophobic fumed silica after the heat treatment may decrease. In this case, the water content of the hydrophobic fumed silica is preferably 0.2% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.05 to 0.1% by mass.
[0132] Commercially available silica can be used as such silica. Examples of commercially available silica include "AEROSIL R974," "AEROSIL RX200," and "AEROSIL 200" manufactured by AEROSIL Japan. Furthermore, silica described in Japanese Patent Application Publication No. 2001-139816 can also be used as the silica.
[0133] Silica can also be prepared by pre-heating the silica and curable organopolysiloxane (A). Pre-heating a portion or all of the silica and curable organopolysiloxane (A) improves the affinity between the two components, thereby suppressing silica aggregation.
[0134] Examples of methods for heat-treating silica and curable organopolysiloxane (A) include treatments at normal pressure or reduced pressure, preferably at 100°C or higher and below the decomposition temperature of the components, more preferably at 100 to 300°C, and even more preferably at 140 to 200°C, for preferably 3 to 30 hours.
[0135] Silica is preferably added to the coating composition as a kneaded product with the curable organopolysiloxane (A). By using a kneaded product of the curable organopolysiloxane (A) and silica, an excessive increase in the viscosity of the coating composition can be suppressed.
[0136] As a method for producing a kneaded product of silica and curable organopolysiloxane (A), for example, there can be mentioned a method described in JP-A-2004-182908.
[0137] When the coating composition of the present embodiment contains an inorganic filler (C), the amount of the inorganic filler (C) relative to 100 parts by mass of the curable organopolysiloxane (A) is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, from the viewpoint of improving the thixotropy of the coating composition and improving the coating film strength and coating film hardness. Furthermore, from the viewpoint of suppressing an excessive increase in the viscosity of the coating composition, the amount is preferably 50 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less.
[0138] When the coating composition of the present embodiment contains an inorganic filler (C), the content of the inorganic filler (C) in the solid content of the coating composition is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 1.5% by mass or more, from the viewpoint of improving the thixotropy of the coating composition and improving the coating film strength and coating film hardness. Furthermore, from the viewpoint of suppressing an excessive increase in the viscosity of the coating composition, it is preferably 50% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and even more preferably 5% by mass or less.
[0139] <Silane coupling agent (D)>
[0140] The antifouling coating composition of the present embodiment may contain a silane coupling agent (D) for the purpose of improving the adhesion of the formed antifouling coating film to the substrate or the primer coating film.
[0141] As the silane coupling agent (D), for example, a compound represented by the following formula (D1) is preferably used.
[0142] [Chemistry 6]
[0143] (R 21 O) w R 22 (3-w) Si-R 23 -Z (D1)
[0144] In formula (D1), R 21 and R 22 Each independently represents an alkyl group, alkenyl group, aryl group, or halogenated alkyl group having 1 to 10 carbon atoms, and is preferably a methyl group or an ethyl group.
[0145] In formula (D1), R 23 It is a divalent hydrocarbon group having 1 to 20 carbon atoms which may be interposed with an amino group (-NR-, R represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms), an ether group (-O-), a sulfide group (-S-), an ester group (-C(=O)-O-), or an amide group (-C(=O)-NR-, R represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms), and is preferably an alkylene group having 4 to 11 carbon atoms interposed with an amino group.
[0146] In formula (D1), Z is a polar group, preferably an amino group, an imino group, a glycidyl group, an isocyanate group, a thiol group, a hydrosilyl group or a (meth)acrylic group, and more preferably an amino group.
[0147] In formula (D1), w is an integer of 2 or 3, and preferably 3.
[0148] Examples of such silane coupling agents (D) include 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-(2-aminoethyl)aminoethyl)aminopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-isocyanatepropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane, and partial condensates thereof may also be used.
[0149] These silane coupling agents (D) may be used alone or in combination of two or more.
[0150] When the antifouling coating composition of the present embodiment contains a silane coupling agent (D), the content of the silane coupling agent (D) in the solid content of the coating composition is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, even more preferably 0.1% by mass or more, and is preferably 5% by mass or less, more preferably 2% by mass or less, even more preferably 0.5% by mass or less, and even more preferably 0.3% by mass or less, from the viewpoint of improving the adhesion of the formed antifouling coating film to the substrate and the primer coating film.
[0151] <Silicone Oil (E)>
[0152] The antifouling coating composition of the present embodiment may contain silicone oil (E) for the purpose of improving the antifouling properties of the formed antifouling coating film.
[0153] As the silicone oil (E), silicone oil represented by the following formula (E1) is preferred.
[0154] [Chemistry 7]
[0155]
[0156] (In formula (E1), R 31 、R 32 Each independently represents a hydrogen atom or an alkyl group, alkenyl group, aryl group, aralkyl group or halogenated alkyl group having 1 to 50 carbon atoms which may have a heteroatom in its structure, R 33 represents a single bond or a divalent hydrocarbon group having 1 to 50 carbon atoms which may be interposed with an amino group, an ether group, a thioether group, an ester group, or an amide group. s represents an integer from 10 to 1000.
[0157] In formula (E1), R 31 、R 32When representing an alkyl group, alkenyl group, aryl group, aralkyl group, or haloalkyl group having 1 to 50 carbon atoms, each of these groups may independently have a heteroatom in the structure, that is, may contain a group having a heteroatom in the structure. Examples of the heteroatom include oxygen, nitrogen, and sulfur, and examples of the group having a heteroatom include an amino group, an amide group, an ether group, an ester group, an alcohol group, a carboxyl group, a thioether group, and a thiol group.
[0158] There are multiple R 31 、R 32 They can be the same or different.
[0159] As silicone oil (E), R 31 and R 32 Silicone oil composed only of alkyl groups, R 31 and R 32 Silicone oil composed of alkyl and aryl groups.
[0160] As R 31 and R 32 Silicone oil (E) composed only of alkyl groups preferably has a plurality of R 31 and R 32 Silicone oil composed entirely of methyl groups (hereinafter referred to as "polydimethylsiloxane (unmodified)"), R 31 and R 32 Silicone oils composed of methyl and other alkyl groups are more preferably silicone oils having an ether group as the other alkyl group. Examples of other alkyl groups having an ether group include -R(C2H4O) a (C3H6O) b R' (herein, R represents an alkylene group having 1 to 20 carbon atoms, R' represents an alkyl group having 1 to 20 carbon atoms, a and b represent integers of 0 to 30, and a+b is an integer greater than 1.) 31 and R 32 The silicone oil (E) composed of a methyl group and an alkyl group having an ether group is called an "ether-modified polydimethylsiloxane".
[0161] As the above R 31 and R 32 Silicone oil (E) composed of alkyl and aryl groups, preferably R 31 and R 32 Silicone oil composed of methyl and phenyl groups (hereinafter also referred to as "phenyl-modified polydimethylsiloxane"), preferably phenyl groups in all R 31 and R 32 The proportion of the silicone oil (phenyl modification rate) is 3 to 50%.
[0162] In formula (E1), R 33It represents a single bond or a divalent hydrocarbon group having 1 to 50 carbon atoms which may be interposed with an amino group, an ether group, a thioether group, an ester group, or an amide group.
[0163] There are multiple R 33 They can be the same or different.
[0164] As R 33 , preferably a single bond. 33 In the case of a divalent hydrocarbon group having 1 to 50 carbon atoms and an ether group interposed therebetween, for example, -R(C2H4O) a (C3H6O) b A group having a chemical structure of R"-(R, R" each independently represents an alkylene group having 1 to 10 carbon atoms, a and b represent integers of 0 to 30, and a+b is an integer of 1 or greater).
[0165] Regarding the viscosity of the silicone oil (E) at 23°C, from the viewpoint of improving the operability during the production of the coating composition, improving the spray atomization and curing properties of the coating composition, and the strength of the formed coating film, it is preferably 10 mPa·s or more, more preferably 20 mPa·s or more, further preferably 40 mPa·s or more, further preferably 60 mPa·s or more, further preferably 80 mPa·s or more, and preferably 10,000 mPa·s or less, more preferably 5,000 mPa·s or less, further preferably 3,000 mPa·s or less, and further preferably 2,000 mPa·s or less.
[0166] In addition, in this specification, the viscosity of the silicone oil (E) at 23°C means the viscosity measured with a Brookfield rotational viscometer.
[0167] The antifouling coating composition of the present embodiment may use the silicone oil (E) alone or in combination of two or more.
[0168] When the antifouling coating composition of the present embodiment contains silicone oil (E), the content of the silicone oil (E) in the solid content of the coating composition is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 3% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, from the viewpoint of improving the antifouling properties of the formed antifouling coating film.
[0169] As the silicone oil (E), commercially available products can be used. Examples of commercially available products include "KF-96-1000cs" (manufactured by Shin-Etsu Chemical Co., Ltd.), which is the aforementioned polydimethylsiloxane (unmodified), and "KF-50-1000cs" (manufactured by Shin-Etsu Chemical Co., Ltd., phenyl modification rate = 5%, kinematic viscosity (25°C): 1000 mm / s) which is the aforementioned phenyl-modified polydimethylsiloxane. 2 / s), "X-22-4272" (manufactured by Shin-Etsu Chemical Co., Ltd.) as the ether-modified polydimethylsiloxane, the R 31 "Ether-modified polydimethylsiloxane in which a portion of the alkyl group is an ether group), "KF-6020" (manufactured by Shin-Etsu Chemical Co., Ltd., the above R 32 Ether-modified polydimethylsiloxane in which a portion of the alkyl group has an ether group, kinematic viscosity (25°C): 180 mm 2 / s), "FZ-2203" (Toray Dow Corning Co., Ltd., the above R 33 "FZ-2160" (manufactured by Dow Corning Toray Co., Ltd., the above R 32 A part of which is a polydimethylsiloxane having a propylene group having an ether group) etc.
[0170] <Acrylic polymer (F) having a hydrophilic group>
[0171] The coating composition of the present embodiment may contain an acrylic polymer (F) having a hydrophilic group for the purpose of improving adhesion inhibition of aquatic organisms (antifouling properties) by imparting good slip properties to the antifouling coating film formed from the coating composition.
[0172] The acrylic polymer (F) having a hydrophilic group used in the coating composition preferably contains a structural unit derived from a monomer having a hydrophilic group, more preferably contains a structural unit derived from a monomer having a hydrophilic group and a structural unit derived from a hydrophobic monomer, and further preferably consists of a structural unit derived from a monomer having a hydrophilic group and a structural unit derived from a hydrophobic monomer.
[0173] The content of the structural unit derived from the monomer having a hydrophilic group in the acrylic polymer (F) having a hydrophilic group is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, even more preferably 10% by mass or more, and particularly preferably 20% by mass or more, and is 100% by mass or less, preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 60% by mass or less, and even more preferably 50% by mass or less.
[0174] It is believed that by providing the acrylic polymer with hydrophilic groups, when the resulting antifouling coating is placed in water, the hydrophilic sites of the acrylic polymer dissolve or swell, gradually migrating to the surface of the antifouling coating, thereby effectively preventing the adhesion of aquatic organisms. It is also believed that due to its acrylic structure, it gradually hydrolyzes, changing its affinity for water, allowing the acrylic polymer to gradually migrate to the surface of the antifouling coating, thereby maintaining antifouling properties for a long time.
[0175] The hydrophilic group of the monomer having a hydrophilic group is preferably an ether group or a hydroxyl group, more preferably an ether group, further preferably a polyether group, and further preferably a polyethyleneoxy group, from the viewpoint of improving the antifouling property and scratch resistance of the antifouling coating film formed.
[0176] As the monomer having a hydrophilic group, from the viewpoint of improving the antifouling property and scratch resistance of the formed antifouling coating film, a monomer having a polyalkylene glycol group and a monomer having a hydroxyl group are preferred, and a monomer having a polyalkylene glycol group is more preferred.
[0177] Specifically, from the viewpoint of improving antifouling properties, at least one selected from polyalkylene glycol (meth)acrylate, hydroxyalkyl (meth)acrylate, alkoxyalkyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 4-(meth)acryloylmorpholine and vinylpyrrolidone is preferred, at least one selected from polyalkylene glycol (meth)acrylate and hydroxyalkyl (meth)acrylate is more preferred, and polyalkylene glycol (meth)acrylate is further preferred.
[0178] Examples of the polyalkylene glycol (meth)acrylate include polyalkylene glycol (meth)acrylates in which one terminal of the polyalkylene glycol is ester-bonded to (meth)acrylic acid directly or through a linking group, and the remaining terminal is a hydroxyl group or an alkoxy group. Polyalkylene glycol (meth)acrylates in which the remaining terminal is an alkoxy group are preferred.
[0179] Among them, polyalkylene glycol (meth)acrylates in which one terminal of the polyalkylene glycol is directly ester-bonded to (meth)acrylic acid are preferred, and polyalkylene glycol (meth)acrylates in which the remaining terminal is an alkoxy group are more preferred.
[0180] The terminal (meth)acrylic acid is preferably acrylic acid or methacrylic acid, and more preferably acrylic acid.
[0181] Examples of the terminal alkoxy group include methoxy, phenoxy, and octyloxy, among which methoxy and phenoxy are preferred, and methoxy is more preferred.
[0182] The polyalkylene glycol constituting the polyalkylene glycol (meth)acrylate is preferably polyethylene glycol, polypropylene glycol, or a copolymer of ethylene glycol and propylene glycol, and more preferably polyethylene glycol.
[0183] The average number of alkylene glycol units constituting the polyalkylene glycol in the polyalkylene glycol (meth)acrylate is preferably 2 or more, more preferably 3 or more, even more preferably 5 or more, and is preferably 25 or less, more preferably 15 or less, even more preferably 12 or less.
[0184] Specific examples of polyalkylene glycol (meth)acrylates include polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, poly(ethylene glycol-butylene glycol) mono(meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, allyloxypoly(ethylene glycol-propylene glycol) mono(meth)acrylate, phenoxypoly(ethylene glycol-propylene glycol) methacrylate, octyloxypoly(ethylene glycol-propylene glycol) mono(meth)acrylate, dodecyloxypolyethylene glycol mono(meth)acrylate, octadecyloxypolyethylene glycol mono(meth)acrylate, and nonylphenoxypolypropylene glycol acrylate, among which methoxypolyethylene glycol mono(meth)acrylate is preferred.
[0185] As the polyalkylene glycol (meth)acrylate, a commercially available item can be used. Examples of such commercially available products include NK Ester AM-90G (methoxy polyethylene glycol #400 acrylate), NK Ester AM-130G (methoxy polyethylene glycol #550 acrylate), NK Ester M-90G (methoxy polyethylene glycol #400 methacrylate), and NK Ester M-230G (methoxy polyethylene glycol #1000 methacrylate) manufactured by Shin-Nakamura Chemical Co., Ltd.; LIGHT ACRYLATE MTG-A (methoxy-triethylene glycol acrylate), LIGHT ACRYLATE EC-A (ethoxy-diethylene glycol acrylate), LIGHT ACRYLATE EHDG-AT (2-ethylhexyl-diethylene glycol acrylate), and LIGHT ESTER 041MA (methoxy polyethylene glycol methacrylate) manufactured by Kyoeisha Chemical Co., Ltd.; and BLEMMER ANP-300 (nonylphenoxy polypropylene glycol acrylate) and BLEMMER AP-400 (polypropylene glycol monoacrylate), BLEMMER 70PEP-350B (polyethylene glycol polypropylene glycol monomethacrylate), BLEMMER 55PET-800 (polyethylene glycol 1,4-butanediol monomethacrylate), BLEMMER 50POEP-800B (octyloxy polyethylene glycol polypropylene glycol methacrylate); VISCOAT#MTG (methoxy polyethylene glycol acrylate) manufactured by Osaka Organic Chemical Industry Co., Ltd., etc.
[0186] Examples of the hydroxyalkyl (meth)acrylate include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate.
[0187] As the hydroxyalkyl (meth)acrylate, a commercially available product can be used. Examples of such commercially available products include LIGHT ESTER HOA(N) (2-hydroxyethyl acrylate), LIGHT ESTER HO-250(N) (2-hydroxyethyl methacrylate), and LIGHT ESTER HOP(N) (2-hydroxypropyl methacrylate) manufactured by Kyoeisha Chemical Co., Ltd.
[0188] Examples of the alkoxyalkyl (meth)acrylate include methoxyethyl (meth)acrylate and the like.
[0189] As the tetrahydrofurfuryl (meth)acrylate, tetrahydrofurfuryl acrylate and tetrahydrofurfuryl methacrylate are preferred, and tetrahydrofurfuryl acrylate is more preferred.
[0190] As 4-(meth)acryloylmorpholine, 4-acryloylmorpholine and 4-methacryloylmorpholine are preferred, and 4-acryloylmorpholine is more preferred.
[0191] Examples of the vinyl pyrrolidone include 1-vinyl-2-pyrrolidone (N-vinyl-2-pyrrolidone), 3-acetyl-1-vinyl-2-pyrrolidone, and 3-benzoyl-1-vinyl-2-pyrrolidone, among which 1-vinyl-2-pyrrolidone is preferred.
[0192] In addition, (meth)acrylic acid can also be mentioned as the monomer having a hydrophilic group.
[0193] The content of the structural unit derived from the hydrophobic monomer in the acrylic polymer (F) having a hydrophilic group is preferably 99% by mass or less, more preferably 97% by mass or less, even more preferably 95% by mass or less, even more preferably 90% by mass or less, and particularly preferably 80% by mass or less, and is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 50% by mass or more.
[0194] It is believed that by including a hydrophobic monomer in the acrylic polymer, high affinity can be achieved with the curable organopolysiloxane (A) and other components of the antifouling coating composition, thereby achieving uniform slip properties on the surface of the antifouling coating film.
[0195] Examples of the hydrophobic monomer include alkyl (meth)acrylates having a linear, branched, or cyclic alkyl group having 1 to 30 carbon atoms, aryl (meth)acrylates having an aromatic group having 6 to 10 carbon atoms, and silicones containing a (meth)acrylate group. Alkyl (meth)acrylates and silicones containing a (meth)acrylate group are preferred, and alkyl (meth)acrylates are more preferred.
[0196] The carbon number of the alkyl group of the alkyl (meth)acrylate is preferably 1 to 30, more preferably 4 to 18, further preferably 4 to 8, and even more preferably 4 to 6.
[0197] The alkyl group is linear, branched, or cyclic, preferably linear or branched, and more preferably branched.
[0198] Specific examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 3,5,5-trimethylhexyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate. Among these, n-butyl (meth)acrylate, isobutyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred.
[0199] The number of carbon atoms in the aromatic group of the aryl (meth)acrylate is preferably 6 or more and 10 or less, more preferably 6 or more and 7 or less.
[0200] Specific examples of the aryl (meth)acrylate include phenyl (meth)acrylate and benzyl (meth)acrylate.
[0201] Examples of the (meth)acrylic group-containing silicone include methacrylic group-containing silicone and acrylic group-containing silicone, and methacrylic group-containing silicone is preferred.
[0202] The silicone containing a (meth)acrylic group is preferably a silicone in which a (meth)acrylic group is bonded to one end of the silicone main chain via a linking group, and a silicone in which a (meth)acrylic group is directly bonded to one end of the silicone main chain. The silicone in which a (meth)acrylic group is bonded to one end of the silicone main chain via a linking group is preferred.
[0203] The above-mentioned linking group is preferably a trimethylene group.
[0204] The silicone main chain is preferably composed of linear or branched dimethyl silicone (polydimethylsiloxane), and more preferably composed of linear dimethyl silicone.
[0205] Furthermore, it is more preferable that an alkyl group having 1 to 6 carbon atoms exists at the terminal on the opposite side to the (meth)acrylic acid group, and it is more preferable that a butyl group exists.
[0206] As silicones containing (meth)acrylate groups, commercially available products can be used. Examples of such commercial products include Silaplane TM-0701T (tris(trimethylsiloxy)silylpropyl methacrylate), Silaplane FM-0711 (dimethylpolysiloxane containing methacrylate groups, number average molecular weight 1000), and Silaplane FM-0721 (dimethylpolysiloxane containing methacrylate groups, number average molecular weight 5000) manufactured by JNC Corporation.
[0207] By including a (meth)acrylic group-containing silicone, the antifouling property of the formed antifouling coating film can be improved.
[0208] The acrylic polymer (F) having a hydrophilic group can be obtained by polymerizing the above-mentioned hydrophilic monomer and hydrophobic monomer. As the polymerization method, a known method using a polymerization initiator can be employed.
[0209] The weight average molecular weight (Mw) of the acrylic polymer (F) having a hydrophilic group is preferably 1,000 or more, more preferably 3,000 or more, even more preferably 5,000 or more, and even more preferably 7,000 or more, and is preferably 30,000 or less, and more preferably 15,000 or less, from the viewpoint of improving the viscosity of the antifouling coating composition and the antifouling properties of the resulting antifouling coating film.
[0210] When the weight average molecular weight (Mw) of the acrylic polymer (F) having a hydrophilic group is within the above range, it is preferable from the viewpoint that good antifouling properties and scratch resistance can be imparted to the formed antifouling coating film.
[0211] When the present composition contains an acrylic polymer (F) having a hydrophilic group, the content thereof in the solid content of the antifouling coating composition is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 3% by mass or more, and is preferably 40% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and even more preferably 5% by mass or less, from the viewpoint of the antifouling properties and damage resistance of the antifouling coating film formed.
[0212] <Antifouling Agent (G)>
[0213] The antifouling coating composition of the present embodiment may contain an antifouling agent (G) for the purpose of improving the antifouling properties of the antifouling coating film to be formed.
[0214] Examples of the antifouling agent (G) include cuprous oxide, cuprous thiocyanate, copper, copper pyrithione, zinc pyrithione, 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitrile (common name: bromopyrrolecarbonitrile), 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one, borane-nitrogen base adducts (pyridinetriphenylborane, 4-isopropylpyridinediphenylmethylborane, etc.), (+ / -)-4-[1-(2,3-dimethylphenyl)ethyl]-1H-imidazole (common name: medetomidine), N,N-dimethyl-N'-(3,4-dichlorophenyl)urea, N-(2,4,6-trichlorophenyl)urea, These antifouling agents include zinc dimethyldithiocarbamate, zinc ethylenebis(dithiocarbamate), zinc 2-methylthio-4-tert-butylamino-6-cyclopropylamino-1,3,5-triazine, 2,4,5,6-tetrachloroisophthalonitrile, zinc bis(dimethyldithiocarbamoyl)ethylenebis(dithiocarbamate), chloromethyl-n-octyl disulfide, N,N-dimethyl-N'-phenyl-(N'-fluorodichloromethylthio)sulfonamide, tetraalkylthiuram disulfide, zinc dimethyldithiocarbamate, zinc ethylenebis(dithiocarbamate), 2,3-dichloro-N-(2',6'-diethylphenyl)maleimide, and 2,3-dichloro-N-(2'-ethyl-6'-methylphenyl)maleimide. These antifouling agents may be used alone or in combination of two or more.
[0215] Among them, from the viewpoint of excellent storage stability and curability of the antifouling coating composition and the antifouling properties of the formed antifouling coating film, cuprous oxide, cuprous thiocyanate, copper, copper pyrithione, zinc pyrithione, bromopyrrolecarbonitrile, 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one, and borane-nitrogen base adducts (pyridinetriphenylborane and 4-isopropylpyridinediphenylmethylborane, etc.) are preferred, and copper pyrithione is more preferred.
[0216] When the antifouling coating composition of the present embodiment contains an antifouling agent (G), the content of the antifouling agent (G) in the solid content of the coating composition is preferably 0.05% by mass or more, more preferably 1% by mass or more, and is preferably 50% by mass or less, more preferably 30% by mass or less, from the viewpoint of improving the antifouling properties of the antifouling coating film formed. When the antifouling coating composition of the present embodiment contains copper pyrithione as the antifouling agent (G), the content of copper pyrithione in the solid content of the coating composition is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, from the viewpoint of improving the antifouling properties of the antifouling coating film formed.
[0217] <Silicone Crosslinking Agent (H)>
[0218] The antifouling coating composition of the present embodiment may contain an organosilicon crosslinking agent (H) for the purpose of improving the curability and coating film strength of the antifouling coating film.
[0219] The organosilicon crosslinking agent (H) is preferably a compound represented by the following formula (H1) and / or a partial condensate thereof.
[0220] R 51 d SiE (4-d) (H1)
[0221] (In formula (H1), R 51 represents a hydrocarbon group having 1 to 6 carbon atoms, Y each independently represents a hydrolyzable group, and d represents an integer of 0 to 2.
[0222] In formula (H1), R 51 Each independently represents a hydrocarbon group having 1 to 6 carbon atoms, and examples thereof include linear or branched alkyl groups such as methyl, ethyl, and propyl, cyclic alkyl groups such as cyclohexyl, alkenyl groups such as vinyl, and aryl groups such as phenyl. Among them, methyl and ethyl are preferred.
[0223] It should be noted that when d is 2, there are multiple R 51 They can be the same or different.
[0224] In formula (H1), each Y independently represents a hydrolyzable group. Examples of the hydrolyzable group include the hydrolyzable groups exemplified in formula (A1). Among these, alkoxy groups and oxime groups are preferred, methoxy groups and ethoxy groups are more preferred as alkoxy groups, and methyl ethyl ketoxime groups and methyl isobutyl ketoxime groups are more preferred as oxime groups.
[0225] d represents an integer of 0 to 2, and is preferably 0 or 1, more preferably 0, when Y is an alkoxy group, from the viewpoint of improving the curability and film strength of the antifouling coating film. d is preferably 1 when Y is an oxime group.
[0226] As the organosilicon crosslinking agent (H), commercially available products can be used. As commercial products, for example, in the case of tetraethyl orthosilicate, "Ethyl Silicate 28" manufactured by Colcoat and "Ethyl Orthosilicate" manufactured by Tama Chemical Industry Co., Ltd. can be cited. In the case of partially hydrolyzed condensates of tetraethyl orthosilicate, "Silicate 40" manufactured by Tama Chemical Industry Co., Ltd. and "WACKER SILICATE TES 40WN" manufactured by Asahi Kasei Wacker Silicone Co., Ltd. can be cited. In the case of alkyltrialkoxysilane, "KBM-13" manufactured by Shin-Etsu Chemical Co., Ltd. can be cited. In the case of vinyltri(methylethylketoxime)silane, "BCA-100" manufactured by Shin-Etsu Chemical Co., Ltd. can be cited.
[0227] When the coating composition of the present embodiment contains an organosilicon crosslinking agent (H), the content of the organosilicon crosslinking agent (H) in the solid content of the coating composition is preferably 0.2% by mass or more, more preferably 1% by mass or more, even more preferably 2% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, from the viewpoint of adjusting the curing rate of the formed coating film and improving the coating film strength.
[0228] <Curing Catalyst (I)>
[0229] The antifouling coating composition of the present embodiment may contain a curing catalyst (I) for the purpose of increasing the curing rate of the formed coating film and improving the strength of the coating film.
[0230] Examples of the curing catalyst (I) include those described in Japanese Patent Application Laid-Open No. 4-106156.
[0231] Specifically, we can cite:
[0232] Tin carboxylates such as tin naphthenate and tin oleate;
[0233] Tin compounds such as dibutyltin diacetate, dibutyltin acetylacetonate, dibutyltin dilaurate, dibutyltin dioleate, dibutyltin oxide, dibutyltin dimethoxy, dibutyltin divalerate, dibutyltin dioctoate, dibutyltin dineodecanoate, dioctyltin dineodecanoate, bis(dibutyltin laurate) oxide, bis(triethoxysiloxy)dibutyltin, bis(dibutyltin acetate) oxide, dibutyltin bis(ethylmalate), and dioctyltin bis(ethylmalate);
[0234] Titanates or titanium chelates such as tetraisopropoxytitanium, tetra-n-butoxytitanium, tetra(2-ethylhexyloxy)titanium, dipropoxybis(acetylacetonate)titanium, isopropoxyoctyl glycol titanium, etc.;
[0235] Organometallic compounds such as zinc naphthenate, zinc stearate, zinc 2-ethyloctoate, iron 2-ethylhexanoate, cobalt 2-ethylhexanoate, manganese 2-ethylhexanoate, cobalt naphthenate, and alkoxyaluminum compounds;
[0236] Lower fatty acid salts of alkali metals such as potassium acetate, sodium acetate and lithium oxalate, etc.
[0237] As the curing catalyst (I), commercially available products can be used, for example, “NEOSTAN U-100” manufactured by Nitto Kasei Co., Ltd. and “K-KAT XK-618” manufactured by King Industries.
[0238] When the coating composition of the present embodiment contains a curing catalyst (I), the content of the curing catalyst (I) in the solid content of the coating composition is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 1% by mass or more, and is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, from the viewpoint of increasing the curing rate of the formed coating film and achieving a good balance with the usable life after preparation of the coating composition.
[0239] <Pigment (J)>
[0240] The coating composition of the present embodiment may contain a pigment (J) other than the aforementioned inorganic filler (C) for the purpose of improving the design and visibility of the coating composition and its coating film.
[0241] The pigment (J) is not particularly limited. Examples thereof include inorganic pigments such as iron oxide, titanium oxide, carbon black, and zinc oxide; and organic pigments such as naphthol red and phthalocyanine blue. From the viewpoint of the production operability, coating operability, storage stability, antifouling properties of the antifouling coating film, and damage resistance of the coating composition, inorganic pigments are preferred. Among them, one or more selected from the group consisting of iron oxide, titanium oxide, carbon black, zinc oxide, aluminum silicate, alumina white, and barium sulfate are preferred. One or more selected from the group consisting of iron oxide, titanium oxide, and carbon black are preferred, and one or more selected from the group consisting of iron oxide and titanium oxide are more preferred.
[0242] Examples of the iron oxide include red iron oxide, yellow iron oxide, and black iron oxide.
[0243] As titanium oxide, any of rutile, anatase, and brookite types can be used. From the viewpoint of the stability of the antifouling coating film and the antifouling coating composition, and the availability, rutile type is preferably used.
[0244] Examples of the organic pigment include naphthol red and phthalocyanine blue.
[0245] When the coating composition contains a pigment (J), the content of the pigment (J) in the solid content of the coating composition is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 5% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, from the viewpoints of the antifouling properties and damage resistance of the antifouling coating film formed from the coating composition, and the production workability, coating workability, and storage stability of the antifouling coating composition.
[0246] On the other hand, when the antifouling coating film of this embodiment is used for applications requiring transparency and light transmittance, it is preferred that the pigment (J) is substantially not contained, or the content of the pigment (J) in the solid content of the coating composition is limited to 0.5% by mass or less.
[0247] <Organic Solvent (K)>
[0248] The antifouling coating composition of the present embodiment may contain an organic solvent (K) for the purpose of maintaining the viscosity of the coating composition low and improving coating properties.
[0249] Examples of the organic solvent (K) include aromatic hydrocarbon organic solvents, aliphatic hydrocarbon organic solvents, alicyclic hydrocarbon organic solvents, ketone organic solvents, and ester organic solvents. Among them, aromatic hydrocarbon organic solvents and ketone organic solvents are preferred.
[0250] Examples of the aromatic hydrocarbon organic solvent include toluene, xylene, and mesitylene.
[0251] Examples of the aliphatic hydrocarbon-based organic solvent include pentane, hexane, heptane, and octane.
[0252] Examples of the alicyclic hydrocarbon organic solvent include cyclohexane, methylcyclohexane, and ethylcyclohexane.
[0253] Examples of the ketone organic solvent include acetylacetone, acetone, methyl ethyl ketone, methyl isobutyl ketone, and dimethyl carbonate.
[0254] Examples of the ester organic solvent include propylene glycol monomethyl ether acetate and the like.
[0255] These organic solvents (K) may be used alone or in combination of two or more.
[0256] When the antifouling coating composition of the present embodiment contains an organic solvent (K), the content of the organic solvent (K) in the coating composition can be appropriately adjusted according to the viscosity of the coating composition, but is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more. From the viewpoint of suppressing sagging during coating, it is preferably 70% by mass or less, more preferably 50% by mass or less, and even more preferably 30% by mass or less.
[0257] <Preferred Embodiments of Antifouling Coating Composition>
[0258] The antifouling coating composition may be a one-component antifouling coating composition in which the above components are made into a single composition, or a multi-component antifouling coating composition in which the above components are made into two or more compositions and mixed before coating. However, from the perspective of preventing deterioration and curing during storage, a multi-component antifouling coating composition is preferred, while from the perspective of coating workability, a one-component antifouling coating composition is preferred.
[0259] Examples of the multi-component antifouling coating composition include a two-component antifouling coating composition and a three-component or higher-component antifouling coating composition. From the viewpoint of coating workability, a two-component antifouling coating composition is preferred, while from the viewpoint of preventing deterioration and solidification during storage, a three-component or higher-component antifouling coating composition is preferred.
[0260] In the case of a multi-liquid antifouling coating composition, the curable organopolysiloxane (A), the silane coupling agent (D), the organosilicon crosslinking agent (H), and the curing catalyst (I) are preferably contained in separate liquids, and the silane coupling agent (D), the organosilicon crosslinking agent (H), and the curing catalyst (I) are more preferably contained in separate liquids.
[0261] The pigment (J), the inorganic filler (C), and the antifouling agent (G) are preferably contained in the same liquid as the curable organopolysiloxane (A).
[0262] In addition, the content of each component in the antifouling coating composition is the content relative to the total amount of all the compositions in the case of a multi-liquid antifouling coating composition.
[0263] <Method for producing antifouling coating composition>
[0264] The antifouling coating composition is preferably produced as follows.
[0265] First, it is preferred to have a step of kneading the curable organopolysiloxane (A) and the inorganic filler (C). Alternatively, heating may be performed during or after kneading. By pre-mixing these, the affinity of the two components is improved, and the aggregation of the inorganic filler (C) and the increase in the viscosity of the coating composition can be suppressed.
[0266] The heating conditions are preferably 100° C. or higher, more preferably 100 to 300° C., and even more preferably 140 to 200° C. The pressure is preferably normal pressure or reduced pressure, and the treatment time is preferably 3 to 30 hours.
[0267] The antifouling coating composition can be obtained by mixing and stirring the above-mentioned components.
[0268] When the antifouling coating composition is a one-component antifouling coating composition, the curable organopolysiloxane (A) and the glycerin condensate ester (B) as essential components and the inorganic filler (C), silane coupling agent (D), silicone oil (E), acrylic polymer having a hydrophilic group (F), antifouling agent (G), organosilicon crosslinking agent (H), curing catalyst (I), pigment (J) and organic solvent (K) as optional components are appropriately added and mixed and stirred to obtain the antifouling coating composition.
[0269] When the antifouling coating composition is a multi-component antifouling coating composition, the curable organopolysiloxane (A), the silane coupling agent (D), the organosilicon crosslinking agent (H), and the curing catalyst (I) are preferably contained in separate liquids. In the case of a three- or more-component antifouling coating composition, the silane coupling agent (D), the organosilicon crosslinking agent (H), and the curing catalyst (I) are preferably further contained in separate liquids.
[0270] Furthermore, it is preferred that the inorganic filler (C), the antifouling agent (G), and the pigment (J) are contained in the same liquid as the curable organopolysiloxane (A).
[0271] The glycerin condensate ester (B) may be contained in any liquid. However, when the coating composition contains the curing catalyst (I), the glycerin condensate ester (B) is preferably contained in the liquid containing the curing catalyst (I).
[0272] In addition, it is preferred that an organic solvent (K) be contained in either liquid.
[0273] The mixing and stirring is preferably performed at 0 to 50°C.
[0274] [Antifouling coating]
[0275] The antifouling coating film of the present embodiment is a film obtained by curing the antifouling coating composition of the present embodiment. Specifically, for example, the antifouling coating film can be obtained by applying the antifouling coating composition of the present embodiment to a substrate or the like and then curing the composition.
[0276] Examples of a method for applying the antifouling coating composition of the present embodiment include known methods using a brush, a roller, a sprayer, and the like.
[0277] The antifouling coating composition applied by the above method is left to stand at 25° C. for about 0.5 to 3 days to cure and form a coating film. The coating composition can be cured while being heated and blown with air.
[0278] The thickness of the antifouling coating film of this embodiment after curing is preferably about 100 to 2000 μm, for example, from the perspective of improving the coating film strength. An example of a method for producing an antifouling coating film of this thickness is a method in which the coating composition is applied one or more times, preferably to a thickness of 30 to 400 μm, more preferably 50 to 300 μm per application.
[0279] The antifouling coating film of the present embodiment can form surface microstructures such as ribs on the coating film surface by contacting the coating film with a mold during formation of the coating film using a method such as that disclosed in International Publication No. 2019 / 189412.
[0280] [Anti-fouling sheet]
[0281] The antifouling sheet of this embodiment has the antifouling coating film of this embodiment.
[0282] The antifouling sheet of the present embodiment may optionally include a base layer, a pressure-sensitive adhesive layer, an intermediate layer, a release layer, and the like in addition to the antifouling coating film.
[0283] The above-mentioned substrate layer is a layer having the function of improving the strength of the antifouling sheet. As long as it is a layer with such a function, it can be used without particular limitation. For example, the substrate layer can be made of resins such as silicone resin, acrylic resin, polyolefin resin, polyethylene resin, polyester resin, polyurethane resin; metals such as stainless steel and aluminum; paper, non-woven fabric, cloth, glass and other materials, or a composite material composed of these materials, a coating film, a film, a sheet, among which, from the aspect of obtaining excellent adhesion even if the coating composition of the present invention is directly applied, a substrate layer made of silicone resin as a material, or a substrate layer obtained by combining the substrate layer with other substrate layers is preferred. As such a substrate layer, it can be a substrate layer having a shielding function that reduces the movement of water and other liquid substances. As such a substrate layer, the substrate layer described as a water vapor barrier layer in Japanese Patent Application Laid-Open No. 2015-224334 can be cited.
[0284] The above-mentioned pressure-sensitive adhesive layer is a layer with the function of sticking the antifouling sheet to the base material. As long as it is a layer with this function, it can be used without particular restriction. As the adhesive forming the pressure-sensitive adhesive layer, for example, acrylic pressure-sensitive adhesives, silicone pressure-sensitive adhesives, natural or synthetic rubber pressure-sensitive adhesives, polyurethane pressure-sensitive adhesives, etc. can be enumerated, and they can also be used in combination. Among them, from the perspective of the design ease of bonding strength, weather resistance, and heat resistance, acrylic pressure-sensitive adhesives are preferred. Silicone pressure-sensitive adhesives that can cope with a wide range of temperature regions, water resistance, chemical resistance are also excellent, and the adhesion to the substrate of silicone is also excellent are also preferred. It should be noted that the antifouling sheet of the present invention also does not have a pressure-sensitive adhesive layer. It can be applied to the adhered object by applying an adhesive when pasting and making it solidify.
[0285] The intermediate layer is a layer having a function of bonding the layers together, and examples thereof include silicone resin-based tie coats.
[0286] The release layer is a layer that temporarily protects the antifouling coating and the pressure-sensitive adhesive layer before the antifouling sheet is attached. Any layer having this function can be used without particular limitation. For example, the release layer can be a release substrate of paper or film coated or modified with a low surface energy compound such as an organic silicone compound, a fluoropolymer, a fluorosilicone, a polyurethane, or a polyolefin. In addition, as the release layer, for example, a release layer that is easily removed by contact with water, such as that disclosed in International Publication No. 2020 / 105630, can be used.
[0287] Examples of the form of the antifouling sheet of the present invention include an antifouling sheet in which a release layer, a pressure-sensitive adhesive layer, a substrate layer, an intermediate layer, an antifouling coating film, and a release layer are laminated in this order; an antifouling sheet in which a release layer, a pressure-sensitive adhesive layer, a substrate layer, an antifouling coating film, and a release layer are laminated in this order; an antifouling sheet in which a release layer, a pressure-sensitive adhesive layer, and an antifouling coating film are laminated in this order; an antifouling sheet in which a release layer, a pressure-sensitive adhesive layer, an intermediate layer, and an antifouling coating film are laminated in this order; and an antifouling sheet in which a substrate layer and an antifouling coating film are laminated in this order.
[0288] As an example of a method for producing such an antifouling sheet, there can be mentioned a method in which a substrate layer is formed, a pressure-sensitive adhesive layer is formed on one side thereof, and then a release layer is laminated thereto, an intermediate layer is formed on the other side, and the antifouling coating composition of the present embodiment is further applied thereon and cured. However, a method in which the antifouling coating composition of the present invention is applied to the substrate layer of a commercially available base tape having a release layer, a pressure-sensitive adhesive layer, and a substrate layer laminated in this order and cured can also be employed.
[0289] The use of such antifouling sheets has the following advantages: it prevents volatile organic solvents from being released into the air during application, allows the formation of an antifouling coating on substrates with low adhesion without the need for primer coating, and allows for easy restoration when antifouling is no longer required.
[0290] An example of the steps for attaching such an antifouling sheet to an adherend includes, for an antifouling sheet comprising a release layer, a pressure-sensitive adhesive layer, a substrate layer, and an antifouling coating layer laminated in this order, peeling off the release layer and attaching the exposed pressure-sensitive adhesive layer to the adherend substrate. Furthermore, as needed, a step may be included in which the ends of the expanded antifouling sheet and the surrounding adherend surface are sealed with a coating or other adhesive tape. For cylindrical adherends, the antifouling sheet itself may be used to press against the antifouling tape, for example by spirally wrapping the sheet.
[0291] [Substrate with antifouling coating and method for producing the same]
[0292] The substrate with an antifouling coating film of the present embodiment has the antifouling coating film or the antifouling sheet of the present embodiment on a substrate.
[0293] The method for producing the substrate with an antifouling coating film of the present embodiment is not particularly limited. For example, the substrate can be produced by a production method comprising the steps of applying or impregnating the antifouling coating composition of the present embodiment onto a substrate to obtain a coated or impregnated product (1), and curing the coated or impregnated product (2).
[0294] In the above step (1), the coating composition can be applied to the substrate by the coating method described above. Furthermore, the impregnation method is not particularly limited, and the substrate can be impregnated with an amount of the coating composition sufficient for impregnation. Furthermore, the method for curing the above-mentioned coating or impregnated material is not particularly limited, and curing can be performed using the same method as used in the production of an antifouling coating film.
[0295] The antifouling coating-film-carrying substrate of the present embodiment can also be obtained by attaching the aforementioned antifouling sheet to a substrate.
[0296] Examples of the substrate include ships (hull plates of large steel ships such as container ships and tankers, fishing boats, FRP ships, wooden boats, and yachts, newly built or repaired ships), fishing supplies (ropes, fishing nets, fishing gear, floats, and buoys, etc.), underwater cables and their protective materials, oil pipelines, water pipes, circulating water pipes, diving suits, underwater goggles, oxygen cylinders, swimsuits, torpedoes, underwater structures such as water supply and drainage outlets of thermal power plants and nuclear power plants, submarine cables, seawater utilization equipment (seawater pumps, etc.), equipment used in and on water (solar power generation panels, measuring instruments, observation windows of equipment, camera lenses, underwater lights, underwater sensors, etc.), ultra-large floating marine structures, bay coastal roads, undersea tunnels, port facilities, and various marine civil engineering works such as canals and aqueducts.
[0297] Among them, the substrate is preferably selected from ships, underwater structures, and fishery materials, more preferably selected from ships and underwater structures, and further preferably ships.
[0298] Furthermore, by substantially not containing the pigment (J) as described above in the above-mentioned applications, or by setting the content of the pigment (J) in the solid content of the coating composition to 0.5% by mass or less, the coating composition can be used for applications requiring transparency and light transmittance, such as underwater glasses, observation windows for measuring instruments and equipment, and camera lenses. This is preferable from the viewpoint that high transparency and light transmittance can impart excellent antifouling properties.
[0299] Examples of the material of the substrate include silicone resins, acrylic resins, polyolefin resins, polyethylene resins such as polyvinyl chloride, (co)polymers of unsaturated monomers such as polystyrene, polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyurethane resins, epoxy resins, polyacetal, polycarbonate, and acetyl cellulose; metals such as iron, aluminum, titanium, and stainless steel; glass, paper, cloth, and the like.
[0300] As the above-mentioned substrate, it can also be used in the form of an underwater antifouling pipe having an antifouling coating of the present embodiment in the outermost layer. As such an antifouling pipe, for example, an antifouling pipe of a form as described in Japanese Patent Application Laid-Open No. 2021-028166 can be cited, for example, the antifouling coating composition of the present invention can be applied to the outer surface of a silicone rubber pipe and cured to obtain an underwater antifouling pipe. Such an antifouling pipe can be used to prevent fouling of underwater cables, etc., for example, cracks are formed along the length direction of the underwater antifouling pipe and wrapped around the underwater cable that is the object of protection, and the cracks are joined with the antifouling coating of the present invention, or bundled with a cable tie that has been subjected to appropriate antifouling treatment and covered around the underwater cable, thereby preventing fouling of the underwater cable.
[0301] [Anti-fouling method]
[0302] The antifouling method of the present embodiment is characterized by using the antifouling coating film of the present embodiment.
[0303] The antifouling coating film obtained by curing the antifouling coating composition of the present embodiment has excellent antifouling properties and can suppress fouling of a substrate covered with the antifouling coating film by aquatic organisms.
[0304] Example
[0305] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.
[0306] [Components of the antifouling coating composition]
[0307] The components used in the coating composition are shown in Tables 1 to 3. The viscosities in Table 1 are all values at 25°C.
[0308] [Table 1]
[0309] Table 1
[0310]
[0311] [Table 2]
[0312] Table 2
[0313]
[0314] *1: Nippon Emulsion Co., Ltd. *2: Nikko Chemical Co., Ltd. *3: Taiyo Chemical Co., Ltd.
[0315] [Table 3]
[0316] Table 3
[0317]
[0318] <Acrylic polymer (F) having a hydrophilic group>
[0319] Synthesis Example 1 (Synthesis of Polymer (F-1))
[0320] The reaction was carried out under normal pressure and a nitrogen atmosphere. 42.86 parts by mass of methyl amyl ketone were added to a reaction vessel equipped with a stirrer, reflux condenser, thermometer, nitrogen inlet tube, and dropping funnel, and the methyl amyl ketone was heated to 100°C while stirring. While maintaining the temperature of the reaction mixture at 100±5°C, a mixture consisting of 40.0 parts by mass of NK Ester AM-90G (methoxypolyethylene glycol acrylate, average number of polyethylene glycol units: 9, manufactured by Shin-Nakamura Chemical Co., Ltd.), 60.0 parts by mass of isobutyl acrylate, and 4.0 parts by mass of 2,2'-azobis(2-methylbutyronitrile) was added dropwise to the reaction vessel over 4 hours. The mixture was then stirred for 2 hours while maintaining the temperature at 100±5°C to obtain a solution of polymer (F-1). The resulting solution had a solids content of 70.3% by mass and a viscosity of 109 mPa·s. The weight-average molecular weight (Mw) of polymer (F-1) was 9100.
[0321] (Solid content of polymer solution)
[0322] The solid content (mass %) was determined by dividing the mass of the solid content obtained by drying the polymer solution at 108° C. and 1 atmosphere for 3 hours by the mass of the polymer solution before drying.
[0323] (Viscosity of polymer solution)
[0324] The viscosity (mPa·s) of the polymer solution at a liquid temperature of 25° C. was measured using an E-type viscometer (TV-25, manufactured by Toki Sangyo Co., Ltd.).
[0325] (Average molecular weight of polymer)
[0326] The weight average molecular weight (Mw) of the polymer was measured using gel permeation chromatography (GPC) under the following conditions.
[0327] (GPC conditions)
[0328] Device: "HLC-8220GPC" (manufactured by TOSOH Corporation)
[0329] Chromatographic columns: "TSKgel SuperH2000" and "TSKgel SuperH4000" (produced by TOSOH Corporation, 6 mm (inner diameter), 15 cm (length)) were connected.
[0330] Eluent: tetrahydrofuran (THF)
[0331] Flow rate: 0.500 mL / min
[0332] Detector: RI
[0333] Column thermostat temperature: 40°C
[0334] Standard material: polystyrene
[0335] Sample preparation method: THF was added to the polymer solution and the solution was filtered with a membrane filter to obtain a sample for GPC measurement.
[0336] [Manufacturing of antifouling coating composition]
[0337] Examples 1 to 12, 14, 15, and Comparative Examples 1 to 4
[0338] The components were mixed and stirred in the amounts (parts by mass) listed in Table 4 to prepare a two-component coating composition consisting of a main component and a curing agent component. The polymer (F-1) was added as a polymer solution in the amounts listed in Table 4. When applying the two-component coating composition, the components were thoroughly stirred and mixed using a disperser before use.
[0339] Example 13
[0340] The components were mixed and stirred according to the amounts (parts by mass) listed in Table 4 to prepare a three-component coating composition consisting of a main component, a curing agent component, and an additive component. When applying the three-component coating composition, the components were thoroughly stirred and mixed using a disperser before use.
[0341] Examples 16 to 19, Comparative Example 5
[0342] A one-component coating composition was prepared by mixing and stirring the components in the amounts (parts by mass) listed in Table 5. When applying the one-component coating composition, the composition was thoroughly stirred and mixed using a disperser before use.
[0343] <Preparation of Test Plates with Coatings>
[0344] Using each coating composition obtained as described above, a test plate with a coating film was produced as follows.
[0345] An epoxy anticorrosion coating ("BANNOH 500" manufactured by China Paint Co., Ltd.) was applied to a sandblasted steel plate (100 mm in length × 70 mm in width × 2.3 mm in thickness) to a thickness of approximately 100 μm after drying (curing), and dried at room temperature (23°C) for 24 hours to form a primer film. Subsequently, a mid-coat coating ("CMP BIOCLEAN TIE-COAT" manufactured by China Paint Co., Ltd.) was applied to a thickness of 100 μm after drying (curing), and dried at room temperature for 24 hours to form a mid-coat film. Subsequently, the coating compositions of Examples 1 to 19 and Comparative Examples 1 to 5 were applied to the mid-coat film at room temperature to a thickness of 200 μm after drying (curing), and dried at room temperature for 1 week to prepare a test plate with a coating film.
[0346] <Stationary Antifouling Evaluation>
[0347] The test panels were immersed in the sea (Hiroshima Bay, Seto Inland Sea) at a depth of 1 meter from the sea surface. Six months later, the ratio of the area of the test panels to which marine organisms adhered (adherence area) was determined by visual observation, with the total area of the antifouling coating of the test panels being taken as 100%. The static antifouling properties were evaluated based on the following criteria. The evaluation results are shown in Table 4 or Table 5 below.
[0348] (Standard for antifouling properties)
[0349] 5: The attachment area of marine organisms is less than 10% of the entire test surface
[0350] 4: The attachment area of marine organisms is more than 10% and less than 30% of the entire test surface
[0351] 3: The attachment area of marine organisms is more than 30% and less than 50% of the entire test surface
[0352] 2: The attachment area of marine organisms is more than 50% and less than 80% of the entire test surface
[0353] 1: The attachment area of marine organisms is more than 80% of the entire test surface
[0354] <Dynamic Antifouling Evaluation>
[0355] The test plate was mounted on a seawater rotor tester located offshore in Kure City, Hiroshima Prefecture, and rotated at a circumferential speed of approximately 15 knots. The test plate was positioned so that the test surface was fully exposed to sunlight, creating conditions conducive to slime formation. Six months later, the ratio of the area of the test plate with slime adhered (adherence area) was determined by visual observation, with the total area of the antifouling coating on the test plate being 100%. Dynamic antifouling properties were evaluated based on the following criteria. The evaluation results are shown in Tables 4 and 5 below.
[0356] (score)
[0357] 5: No mucus adhesion
[0358] 4: The adhesion area of mucus is more than 20% and less than 40% of the entire test surface
[0359] 3: The adhesion area of mucus is more than 40% and less than 60% of the entire test surface
[0360] 2: The adhesion area of mucus is more than 60% and less than 80% of the entire test surface
[0361] 1: The adhesion area of mucus is more than 80% of the entire test surface
[0362] [Table 4]
[0363]
[0364] [Table 5]
[0365] Table 5
[0366]
[0367] <Preparation and Evaluation of Antifouling Sheets and Substrates with Antifouling Sheets>
[0368] "Silicone Rubber Adhesive Tape No. 9013" manufactured by Teraoka Seisakusho Co., Ltd. (having a laminated structure of acrylic adhesive, polyester film, and silicone rubber; total thickness 0.1 mm, adhesive strength 19 N / width 25 mm) was cut into 6 cm x 12 cm pieces. The release surface of a release film (50 μm thick silicone-treated PET film, "SP-PET-O1-50-BU" manufactured by Mitsui Chemicals, Tohcello Co., Ltd.) was attached to the surface with the acrylic adhesive. The coating composition of Example 7 was then applied to the surface with the silicone rubber to a thickness of 200 μm after drying (curing). The tape was then dried at room temperature for one week to produce an antifouling sheet. This antifouling sheet comprises, in this order, the release film as a release layer, the acrylic adhesive as a pressure-sensitive adhesive layer, the polyester film and silicone rubber as base layers, and an antifouling coating film formed from the antifouling coating composition of Example 7 as an antifouling coating film. The antifouling tape prepared in this manner was then affixed to the center of a 7 cm x 15 cm, 2 mm thick vinyl chloride plate, creating a test plate with an antifouling sheet. This test plate was then immersed in real seawater. Three months after the start of immersion, observation revealed that the exposed vinyl chloride plate, where the antifouling sheet was not attached, had become stained by algae. However, the antifouling sheet showed no adhesion, peeling, cracking, or other visual abnormalities, and remained consistent with deformation of the substrate. The present invention enables the production of an antifouling tape that can easily impart antifouling properties to a wide variety of substrates, including various plastics.
[0369] As is apparent from the results of Examples and Comparative Examples, the coating composition of the present invention can form an antifouling coating film having excellent antifouling properties.
Claims
1. An antifouling coating composition comprising a curable organopolysiloxane A and a glycerol condensate ester B represented by the following formula (1): In the formula (1), n is an integer of 2 to 20, and each R independently represents a hydrogen atom or R 1 C(=O)-, at least one R is R 1 C(=O)-,R 1 It represents a monovalent hydrocarbon group having 7 to 23 carbon atoms.
2. The antifouling coating composition according to claim 1, wherein The R 1 Contains branched hydrocarbon groups.
3. The antifouling coating composition according to claim 1, wherein The R comprises an isostearyl group.
4. The antifouling coating composition according to claim 1, wherein At least one R is a hydrogen atom.
5. The antifouling coating composition according to claim 1, wherein The content of the glycerin condensate ester B in the solid content of the antifouling coating composition is 1% by mass or more and 20% by mass or less.
6. The antifouling coating composition according to claim 1, wherein The curable organopolysiloxane A is a compound represented by the following formula (A1): In formula (A1), R 11 and R 13 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aralkyl group or a halogenated alkyl group having 1 to 16 carbon atoms, and R 12 Each independently represents a hydroxyl group or a hydrolyzable group, r represents an integer of 1 to 3, and p represents 10 to 10,000.
7. The antifouling coating composition according to claim 1, wherein The content of the curable organopolysiloxane A in the solid content of the antifouling coating composition is 50% by mass or more and 99% by mass or less. The antifouling coating composition according to claim 1 , further comprising an inorganic filler C.
9. The antifouling coating composition according to claim 8, wherein The inorganic filler C is silica, and the silica is blended into the antifouling coating composition in the form of a kneaded product with the curable organopolysiloxane A. 10 . The antifouling coating composition according to claim 1 , further comprising a silane coupling agent D. 11 . The antifouling coating composition according to claim 1 , further comprising at least one selected from the group consisting of silicone oil E and an acrylic polymer F having a hydrophilic group.
12. An antifouling coating film formed by curing the antifouling coating composition according to any one of claims 1 to 11.
13. An antifouling sheet, It has the antifouling coating film according to claim 12.
14. A substrate with an antifouling coating, The antifouling coating film according to claim 12 is provided on a substrate.
15. The substrate with an antifouling coating according to claim 14, wherein The substrate is selected from ships, underwater structures and fishery materials.
16. A method for producing a substrate with an antifouling coating, the method comprising: Step 1: coating or impregnating a substrate with the antifouling coating composition according to any one of claims 1 to 11 to obtain a coated or impregnated product; and Step 2 of curing the coated or impregnated material.
17. An antifouling method using the antifouling coating film according to claim 12.
Citation Information
Patent Citations
Curable composition, composition for coating, coating material, stainproofing coating material, its cured product, and method of rendering substrate antifoulancy
JP2001139816A
Method for producing liquid silicone composition
JP2004182908A
Adhesive tape for preventing aquatic biofouling
JP2015224334A
Underwater antifouling pipe
JP2021028166A
Antifouling coating film and method of manufacturing same, water contacting structure with antifouling coating film, and antifouling tape and method of manufacturing same