Molten Al-Zn-based plated steel sheet and method for producing same

By adjusting the composition and thermal history conditions of the coated film, the crack problem of molten Al-Zn-type coated steel plates during bending processing is solved, and its high corrosion resistance and bending processing performance in building components is achieved, which meets the needs of the above-mentioned Strict application requirements.

CN119032194APending Publication Date: 2024-11-26JFE GALVANIZING & COATING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093282.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2022-04-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The molten Al-Zn-type plated steel plate is prone to cracks during bending processing, causing the coating protective layer to become thinner or penetrated, reducing its corrosion resistance. The prior art is still not enough to meet the construction components under stricter bending processing conditions. need.

Method used

By adjusting the composition and thermal history conditions of the plated film, the fineness of Zn precipitates and the softening of dendrites are inhibited, the striped structure of Al-Zn eutectics is eliminated, and the thickness of the interface alloy layer is controlled to ensure that the coating film is Excellent bending processability and corrosion resistance.

Benefits of technology

It achieves stable and excellent bending processability and corrosion resistance under stricter bending processing conditions, and meets the high requirements of building components. It is specifically manifested as improving the plated steel plates when there is no crack in the "T bending" test. Corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032194A_ABST
    Figure CN119032194A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a molten Al-Zn-based plated steel sheet which is stable and has excellent bending workability and corrosion resistance in a bent part; and a method for producing the same. In order to achieve the purpose, the present invention is a molten Al-Zn plated steel sheet having a plating film and an interface alloy layer, the plating film having a composition containing 45-65 mass% of Al and 1.0-3.0 mass% of Si, with the remainder comprising Zn, Fe, and unavoidable impurities, a molten Al-Zn-based plated steel sheet comprising a base steel sheet and a plating film formed on the base steel sheet, and an interface alloy layer formed on the interface side with the base steel sheet of the plating film and comprising Fe, Al, Si, Zn and unavoidable impurities, characterized in that the plating film has dendritic crystals mainly comprising primary Al crystals comprising a matrix of an alpha-Al phase and a precipitate of Zn, and dendritic crystal gaps comprising an Al-Zn eutectic crystal, the Zn content in the matrix is 30 mass% or less, and the thickness of the interface alloy layer is 1 [mu] m or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a hot-dip Al-Zn-based plated steel sheet having excellent bending workability and corrosion resistance of a bent portion, and a method for producing the same. Background Art

[0002] It is known that molten Al-Zn type plated steel sheets also show high corrosion resistance in molten galvanized steel sheets because they can take into account the sacrificial corrosion resistance of Zn and the high corrosion resistance of Al. Therefore, molten Al-Zn type plated steel sheets are mostly used in building materials such as roofs or walls that are exposed to the outdoors for a long time, guardrails, wiring and piping, sound insulation walls and other civil engineering fields. In particular, the requirements for materials with excellent corrosion resistance and maintenance-free materials in more severe use environments such as acid rain caused by air pollution, the spread of snow-melting agents for preventing roads from freezing in snowy areas, and the development of coastal areas are constantly increasing. Therefore, in recent years, the demand for molten Al-Zn type plated steel sheets has continued to increase.

[0003] Here, the coating film of the molten Al-Zn type plated steel sheet is composed of a main layer and an interface alloy layer existing at the interface between the base steel sheet and the main layer, and the main layer is mainly composed of a portion (dendritic portion of the α-Al phase) supersaturated with Zn and Al undergoing dendrite solidification and a portion (interdendritic gap) of the remaining dendrites, and has a structure in which the α-Al phase is stacked in a plurality of layers in the film thickness direction of the coating film. Due to this characteristic film structure, the corrosion path from the surface becomes complicated, so it is difficult for corrosion to easily reach the base steel sheet, and the molten Al-Zn type plated steel sheet can achieve more excellent corrosion resistance than the molten galvanized steel sheet with the same thickness of the coating film.

[0004] However, although the molten Al-Zn type plated steel sheet has excellent corrosion resistance, it has the following problems: its plated film is harder than the molten galvanized steel sheet and has poor bending processability. Therefore, when the steel sheet is bent, cracks (ruptures) are easily generated on the plated film at the front end of the bending process. Needless to say, such cracks damage the appearance. The cracks will reach the middle of the plated film, which will cause the thickness of the plated protective layer in this part to become thinner, or the cracks will penetrate the plated film and cause the base steel sheet to be exposed, which will become the reason why the excellent corrosion resistance originally possessed by the molten Al-Zn type plated steel sheet is significantly reduced in the bending process.

[0005] Therefore, various attempts have been made to improve the bending workability of molten Al—Zn-based plated steel sheets.

[0006] For example, there is a technique of applying a predetermined heat history to a molten Al—Zn-based plated steel sheet after plating to attempt to improve the bending workability (for example, refer to Patent Documents 1 and 2).

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent No. 3654521

[0010] Patent Document 2: Japanese Patent Application Publication No. 2013-245355 Summary of the invention

[0011] Technical problem to be solved by the invention

[0012] In the technology of applying a heat history to a molten Al-Zn-based plated steel sheet as in Patent Documents 1 and 2, the plated film can be softened and the bending workability can be improved to some extent.

[0013] However, the bending workability improved by the techniques of Patent Documents 1 and 2 is not sufficient when a more severe bending process is performed, and if the techniques are applied to various building components, it is expected that the bending workability and the corrosion resistance of the processed portion will be further improved. Furthermore, it is also expected that a technique that can more reliably (stably) improve the bending workability and the corrosion resistance of the processed portion will be developed.

[0014] In view of the above circumstances, an object of the present invention is to provide a hot-dip Al—Zn-based plated steel sheet having stable bending workability and excellent corrosion resistance of a bent portion, and a method for producing the same.

[0015] Technical means for solving technical problems

[0016] In order to solve the above-mentioned problems, the inventors of the present application studied a molten Al-Zn plated steel sheet having a plated film (the plated film has the following composition: contains 45 mass% to 65 mass% Al and 1.0 mass% to 3.0 mass% Si, and the remainder is composed of Zn, Fe and inevitable impurities). As a result, it was found that the plated film has: dendrites mainly composed of Al primary crystals, and dendrite gaps containing Al-Zn eutectics, wherein in the Al primary crystals, the Zn precipitates dispersed in the matrix of the α-Al phase are finely divided into 100 nm or less. Focusing on the influence on the hardening of the dendrites, by suppressing the Zn content in the matrix to a low level, it is possible to suppress the refinement and increase of the above-mentioned Zn precipitates while seeking to soften the dendrites, thereby achieving stable and excellent bending workability and corrosion resistance of the processed part.

[0017] In addition, it was found that the precipitation of Zn in the above-mentioned Al primary crystals is closely related to the conditions of the thermal history after the formation of the plating film. With respect to the thermal history after the formation of the plating film, the maximum reached temperature, the heating time, and the cooling time are optimized, thereby suppressing the Zn content in the above-mentioned matrix to a low level, thereby obtaining a molten Al-Zn plated steel sheet having excellent bending workability and corrosion resistance of the processed portion.

[0018] Furthermore, it was found that in the Al-Zn eutectic, there is a structure in which Al parts and Zn parts are alternately arranged in stripes (hereinafter referred to as "striped structure"), and when its period is less than 2 μm, with the aim of reducing the bending workability of the molten Al-Zn plated steel sheet, by eliminating the striped structure, excellent bending workability and corrosion resistance of the processed part can be achieved.

[0019] In addition, it was found that the bending workability can be further improved by suppressing the thickness of the interface alloy layer having a high hardness to 1 μm or less.

[0020] In addition, the so-called excellent bending workability mentioned in the present invention is a practically sufficient bending workability. When evaluated by "T bending", a minimum of "6T crack-free" is required, and preferably "4T crack-free" is required. In addition, the so-called "T bending" is a 180° bending test performed in a state where the thickness of the steel plate is clamped. For example, if it is a "6T bending", six plates of the same thickness are clamped on the inside of the target material and bent at 180°. At this time, the so-called "crack-free" means that no cracks are observed when the outer front end of the bending portion is observed at 10 times using a magnifying glass. In addition, the bending test is a bending test according to the adhesion test of the plating described in JIS G3321 (2019).

[0021] Incidentally, the bending workability of a common molten Al-Zn type plated steel sheet also depends on the conditions of the plated film, but is often "12T crack-free" or higher, and even "10T bending" does not achieve "crack-free".

[0022] The present invention has been accomplished based on the above findings, and the gist of the present invention is as follows.

[0023] 1. A molten Al-Zn plated steel sheet, characterized in that:

[0024] The invention relates to a steel sheet having a plated film and an interface alloy layer, wherein the plated film has the following composition: contains 45 mass % to 65 mass % of Al and 1.0 mass % to 3.0 mass % of Si, and the remainder is composed of Zn, Fe and inevitable impurities, and the interface alloy layer is formed on the interface side between the plated film and the base steel sheet, and contains Fe, Al, Si, Zn and inevitable impurities,

[0025] The plated film has dendrites mainly composed of Al primary crystals and interdendritic gaps containing Al-Zn eutectics.

[0026] The Al primary crystals include a matrix of an α-Al phase and Zn precipitates, and the Zn content in the matrix is ​​30 mass % or less.

[0027] The thickness of the interface alloy layer is less than 1 μm.

[0028] 2. The molten Al—Zn-based plated steel sheet according to item 1 above, wherein an average value of the maximum diameter of the Zn precipitates in the Al primary crystals is 100 nm or more.

[0029] 3. The molten Al-Zn based plated steel sheet described in 1 or 2 above is characterized in that the Al-Zn eutectic in the interdendritic gap does not have a striped structure with a period of 2 μm or less.

[0030] 4. A method for producing a molten Al-Zn-based plated steel sheet, which is the method for producing a molten Al-Zn-based plated steel sheet described in any one of 1 to 3, characterized in that it comprises:

[0031] A step of forming a plating film on a base steel sheet, wherein the plating film has a composition comprising 45 mass % to 65 mass % of Al and 1.0 mass % to 3.0 mass % of Si, with the remainder being Zn, Fe and inevitable impurities; and

[0032] After forming the plating film, a step of providing the steel sheet with a thermal history having a maximum temperature of 150° C. to 277° C.,

[0033] In the step of imparting the thermal history, the cooling time from the highest reached temperature to 150° C. is set to less than two hours, and the cooling time from 150° C. to room temperature is set to more than three hours.

[0034] Effects of the Invention

[0035] According to the present invention, it is possible to provide a hot-dip Al—Zn-based plated steel sheet having stable bending workability and excellent corrosion resistance of a bent portion, and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] [ Figure 1 ] is the equilibrium state diagram of the Al-Zn binary system.

[0037] [ Figure 2 ] is a graph showing the Zn content in the matrix of the α-Al phase, the average value of the maximum diameter of Zn precipitates in the Al primary crystals, and a photograph obtained by observing the cross-section of the Al primary crystals for the samples of the molten Al-Zn plated steel sheets of Comparative Example 1 and Example 14 of the present invention.

[0038] [ Figure 3 ] are photographs obtained by observing the cross-sections of the plating films of the samples of the molten Al-Zn type plated steel sheets of Comparative Example 1, Invention Example 14 and Comparative Example 22.

[0039] [ Figure 4 ] are graphs showing the evaluation results of the corrosion resistance of the bent portions of the samples of the molten Al-Zn type plated steel sheets of Comparative Example 1 and Example 14 of the present invention, and photographs obtained by observing the 1T bent portions. DETAILED DESCRIPTION

[0040] (Molten Al-Zn type plated steel sheet)

[0041] The hot-dip Al—Zn-based plated steel sheet of the present invention has a plated film on the surface of the steel sheet.

[0042] The plated film has a composition of 45 mass % to 65 mass % Al and 1.0 mass % to 3.0 mass % Si, with the remainder substantially consisting of Zn, Fe and inevitable impurities. The plated film of the hot-dip plated steel sheet can achieve good corrosion resistance due to the above composition.

[0043] The plated film is composed of an interface alloy layer present on the interface side with the base steel sheet and a main layer present on the interface alloy layer.

[0044] The Al content in the plating film is 45 to 65% by mass, preferably 50 to 60% by mass, from the viewpoint of balance between corrosion resistance and handling.

[0045] If the Al content in the plated film is at least 45% by mass, dendrite solidification of Al primary crystals will occur, and a structure in which the dendrite solidification structure is stacked in the film thickness direction of the plated film can be obtained. By adopting a structure in which the dendrite solidification structure is stacked in the film thickness direction of the plated film, the corrosion path of the plated film becomes complicated, and the corrosion resistance can be improved. In addition, the more the dendrites are stacked, the more complicated the corrosion path becomes, and the more difficult it is for corrosion to easily reach the base steel plate, thereby improving the corrosion resistance.

[0046] On the other hand, if the Al content in the plating film exceeds 65 mass %, almost all Zn present in the dendrites is taken into the structure of Al primary crystals as a solid solution, and the dissolution reaction of Al primary crystals during corrosion progress cannot be suppressed, resulting in deterioration of corrosion resistance.

[0047] Si in the plating film is added for the purpose of suppressing the growth of an interface alloy layer generated at the interface with the base steel sheet and preventing the adhesion between the plating film and the base steel sheet from being deteriorated.

[0048] In the case of the molten Al-Zn type plated steel sheet of the present invention, if the steel sheet is immersed in an Al-Zn type plating bath containing Si, the Fe on the surface of the steel sheet reacts with the Al or Si in the plating bath to form an alloy, and Fe-Al type and / or Fe-Al-Si type intermetallic compounds (forming an interface alloy layer) are generated in layers at the interface of the base steel sheet / plating film. At this time, since the growth rate of Fe-Al-Si type alloys is slower than that of Fe-Al type alloys, the higher the ratio of Fe-Al-Si type alloys, the more the growth of the overall alloy phase can be suppressed. Therefore, the Si content in the plating film is required to be 1.0 mass% or more.

[0049] On the other hand, the remaining Si that is not consumed in the formation of the interface alloy layer is precipitated as a Si phase in the plated film. The Si phase is electrochemically expensive compared to the Al primary crystal or the Al-Zn eutectic, and acts as a cathode, thereby promoting the corrosion of the plated film and reducing the corrosion resistance. Specifically, if the Si content in the plated film exceeds 3% by mass, not only the growth inhibition effect of the alloy phase described above is saturated, but also the amount of the Si phase increases, thereby promoting corrosion, so the Si content is set to 3.0% by mass or less.

[0050] From the same viewpoint, the Si content in the plated film is more preferably 2.5 mass % or less.

[0051] Furthermore, the plated film contains Zn, Fe, and inevitable impurities.

[0052] Among these components, Fe is a component that is inevitably contained in the coating film due to dissolution of the steel sheet or the equipment in the bath in the coating bath, or a component that is supplied by diffusion from the base steel sheet when the interface alloy layer is formed. It is a component that is inevitably contained in the coating film. Regarding Fe in the coating film, it is impossible to distinguish and quantify Fe taken from the base steel sheet and Fe dissolved from the coating bath. The Fe content in the coating film is generally about 0.3 mass% to 2.0 mass%.

[0053] In addition, examples of inevitable impurities other than Fe include Cr, Ni, Cu, and the like.

[0054] The total content of Fe and the inevitable impurities is not particularly limited, but if contained in excess, various properties of the plated steel sheet may be affected. Therefore, the total content is preferably 5.0 mass % or less, more preferably 3.0 mass % or less.

[0055] In addition, in the molten Al-Zn type plated steel sheet of the present invention, from the viewpoint of being able to improve the stability of corrosion products and delay the progress of corrosion, the plated film may further contain a total of 0.01 mass% to 10 mass% of one or more selected from Mg, Cr, Mn, V, Mo, Ti, Ca, Ni, Co, Sb and B. The reason for setting the total content of the above components to 0.01 mass% to 10 mass% is that a sufficient corrosion delay effect can be obtained and the effect will not be saturated.

[0056] In addition, from the viewpoint of satisfying various properties, the coating weight of the plated film is preferably 45 g / m per single side. 2 ~120g / m 2 The reason is that the coating weight is 45 g / m 2 In the above case, sufficient corrosion resistance can be obtained for applications requiring long-term corrosion resistance such as building materials. In addition, the coating weight of the plating film is 120 g / m 2 In the following cases, it is possible to suppress the occurrence of plating cracks during processing and achieve excellent corrosion resistance.

[0057] From the same viewpoint, the coating weight of the plated film is more preferably 45 g / m 2 ~100g / m 2 .

[0058] Here, the amount of the coating film can be derived, for example, by dissolving and peeling off a specific area of ​​the coating film using a mixed solution of hydrochloric acid and hexamethylenetetramine as specified in JIS H0401:2013, and calculating the weight difference of the steel sheet before and after peeling. In order to obtain the coating adhesion amount of each side by this method, the coating surface of the non-target side may be sealed with an adhesive tape to prevent the coating surface of the non-target side from being exposed, and then the above-mentioned dissolution may be performed.

[0059] In addition, regarding the composition of the plated film, for example, the plated film can be immersed in hydrochloric acid or the like to dissolve it, and the solution can be confirmed by ICP emission spectrometry or atomic absorption spectrometry. This method is only an example, and any method can be used as long as it is a method that can accurately quantify the composition of the plated film, and there is no particular limitation.

[0060] In addition, the coating film of the molten Al-Zn-based plated steel sheet obtained by the present invention has substantially the same composition as the coating bath as a whole. Therefore, the composition of the coating film can be controlled with high accuracy by controlling the coating bath composition.

[0061] In addition, the interface alloy layer in the plated film is a layer in the plated film that exists at the interface with the base steel sheet and is a layered interface alloy layer containing Fe, Al, Si, Zn and inevitable impurities. As described above, the interface alloy layer is inevitably formed by the alloying reaction between Fe on the surface of the base steel sheet and Al or Si in the plating bath.

[0062] Since the interface alloy layer is hard and brittle, it will become the starting point of cracks during processing when it grows thicker, so it needs to be as thin as possible. Therefore, in the molten Al-Zn type plated steel sheet of the present invention, the thickness of the interface alloy layer is required to be less than 1 μm, preferably less than 0.8 μm. If the thickness of the interface alloy layer exceeds 1 μm, the bending workability is reduced.

[0063] In addition, regarding the interface alloy layer, when the cross section of the plated film is observed in three or more viewing fields using a scanning electron microscope (SEM) or the like, the average of the measured values ​​of the average thickness of the interface alloy layer present in each viewing field is taken.

[0064] In addition, there is no particular limitation on the method for reducing the thickness of the interface alloy layer. For example, there can be mentioned a method of adjusting the Si content in the plated film as described above, or a method of adjusting the cooling time when a thermal history is given after forming the plated film as described below.

[0065] Here, in the molten Al-Zn based plated steel sheet of the present invention, the plated film has dendrites and interdendritic gaps, the dendrites are mainly composed of Al primary crystals, and the interdendritic gaps contain Al-Zn eutectics.

[0066] Furthermore, in the molten Al-Zn based plated steel sheet of the present invention, the Al primary crystals are characterized by having Zn precipitates in a matrix of an α-Al phase, and the Zn content in the matrix is ​​30 mass % or less.

[0067] In the matrix of the α-Al phase, if Zn is supersaturated (in a state where the Zn content exceeds 30% by mass) and solidified in a solid solution state, the hardness increases due to the solid solution strengthening of Zn, so the elongation decreases and the bending workability decreases. Therefore, in the present invention, by limiting the Zn content in the matrix to 30% by mass or less, the solid solution strengthening of the Al primary crystal is suppressed, the bending workability of the molten Al-Zn type plated steel sheet is improved, and the corrosion resistance of the processed part is further improved. In addition, since the finer the Zn precipitate, the more significant the reduction in bending workability caused by precipitation strengthening, the growth of Zn precipitates can also be promoted by making the Zn content in the matrix of the α-Al phase less than 30% by mass. In addition, the so-called Zn content in the matrix is ​​the content of Zn contained in the matrix, and does not include the content of precipitated / separated Zn (Zn precipitate).

[0068] From the same viewpoint, the Zn content in the matrix is ​​preferably 25 mass % or less, more preferably 20 mass % or less.

[0069] The so-called Zn precipitate is a granular precipitate with Zn as the main component, but in the present invention, the spatial resolution of the ultra-low accelerating voltage scanning electron microscope (Ultra Low Accelerating Voltage Scanning Electron Microscope, hereinafter referred to as "ultra-low accelerating SEM") used for observation is about 30 nm, and Zn precipitates smaller than this cannot be observed. Therefore, precipitates having a diameter of 30 nm or more are regarded as Zn precipitates.

[0070] Regarding the Al primary crystals, when Zn precipitates are dispersed in the matrix of the α-Al phase, as described above, there is a tendency for the bending workability to decrease due to precipitation strengthening, and the finer the precipitates, the more significant this tendency is. Therefore, it is advantageous to grow the Zn precipitates significantly for the bending workability. Specifically, the average value of the maximum diameter of the Zn precipitates in the Al primary crystals is preferably 100 nm or more.

[0071] In addition, the so-called average value of the maximum diameter of the Zn precipitate is, for example, when observing the Al primary crystal in three or more fields of view by extremely low acceleration SEM (acceleration voltage 3 kV, magnification of 20000 times or more), the long diameter of the precipitate mainly composed of Zn existing in each field of view is measured at 10 points in descending order, and the value obtained by taking the average of these measured values.

[0072] In addition, the plated film has interdendritic gaps containing Al-Zn eutectic. The interdendritic gaps may contain a simple Si phase in addition to the Al-Zn eutectic.

[0073] The Al-Zn eutectic constituting the interdendritic gap is composed of an Al portion and a Zn portion. When the Al-Zn eutectic is heated to 277°C or higher, the Zn solid solubility of the Al portion increases, and the Zn portion is almost solid-dissolved, thereby becoming an Al portion that is more supersaturated with Zn. Thereafter, when the Al-Zn eutectic is cooled, it changes again to an Al-Zn eutectic below 277°C, and at this time, the Al-Zn eutectic has a striped structure in which the Al portion and the Zn portion are alternately arranged in stripes.

[0074] Furthermore, the inventors of the present application conducted research and found that, although the mechanism is still uncertain, the striped structure of the Al-Zn eutectic reduces the bending workability of the molten Al-Zn plated steel sheet, especially when the period of the stripes of the striped structure is as small as less than 2μm, the reduction in bending workability is particularly significant.

[0075] Therefore, from the viewpoint of further improving the bending workability of the molten Al-Zn type plated steel sheet of the present invention and the corrosion resistance of the processed portion, it is preferred that there is no striped structure with a period of less than 2 μm in the Al-Zn eutectic in the interdendritic gap. In addition, there is no particular limitation on the lower limit of the striped period of the striped structure. However, according to the performance of the measuring device described later, it is difficult to confirm the existence of the striped structure when the period is less than 30 nm. Therefore, in the present invention, the striped structure with a period of more than 30 nm is regarded as a striped structure.

[0076] The striped structure of the Al-Zn eutectic can be measured by ultra-low acceleration SEM (acceleration voltage 3 kV) as with the Zn precipitates in the Al primary crystal. In an SEM with a high acceleration voltage, for example, an acceleration voltage of 15 kV or more, the striped structure of the Al-Zn eutectic with a stripe period as small as 2 μm or less cannot be detected, but in the present invention, the presence or absence can be confirmed by observation using an ultra-low acceleration SEM. In addition, since the Zn precipitates and the striped structure of the Al-Zn eutectic are finer than the striped structure generated when the thermal history is applied, the presence or absence of these factors is not taken into account in the observation using an acceleration voltage of 15 kV, for example.

[0077] The method for controlling the Zn content in the matrix, the maximum diameter of Zn precipitates, and the presence or absence of a striped structure with a period of 2 μm or less is not particularly limited, and can be appropriately controlled by optimizing production conditions and the like.

[0078] For example, as described later, by determining the composition of the plating bath and optimizing the conditions of the thermal history after the plating film is formed, the Zn content in the matrix, the maximum diameter of Zn precipitates, and the presence or absence of a striped structure with a period of 2 μm or less can be controlled.

[0079] In the hot-dip Al-Zn-based plated steel sheet of the present invention, a coating film may be formed directly on the plated film or through an intermediate layer.

[0080] In addition, the type of the coating film and the method for forming the coating film are not particularly limited and can be appropriately selected according to the required performance. For example, the forming methods include roller coating, curtain coating, spraying, etc. After the coating containing the organic resin is applied, the coating film can be formed by heating and drying by means of hot air drying, infrared heating, induction heating, etc.

[0081] In addition, the intermediate layer is not particularly limited as long as it is a layer formed between the plated film of the molten-plated steel sheet and the coating film. For example, a chemical conversion film, an adhesive layer or other primer can be cited. The chemical conversion film can be formed, for example, by applying a chromate treatment solution or a chromium-free chemical conversion treatment solution, and performing a chromate treatment or a chromium-free chemical conversion treatment at a temperature of 80 to 300° C. without water washing. These chemical conversion films can be either single-layer or multi-layer. In the case of multi-layer, multiple chemical conversion treatments can be performed in sequence.

[0082] (Method for producing molten Al-Zn-based plated steel sheet)

[0083] The method for producing a molten Al-Zn based plated steel sheet of the present invention comprises: a step of forming a plated film on a base steel sheet; and a step of providing a thermal history to the steel sheet after the plated film is formed.

[0084] The method for forming the plated film on the base steel sheet is not particularly limited, and can be produced, for example, by washing, heating, and immersing the base steel sheet in a plating bath using a continuous hot-dip plating device.

[0085] In the heating step of the base steel sheet, recrystallization annealing is performed to control the structure of the base steel sheet itself. At the same time, heating in a reducing atmosphere such as a nitrogen-hydrogen atmosphere is effective to prevent oxidation of the steel sheet and reduce trace oxide films on the surface.

[0086] Furthermore, there is no particular limitation on the type of the base steel plate or the composition of the steel. Cold-rolled steel plate or hot-rolled steel plate can be used appropriately according to the required performance or specifications. As the composition of the steel, for example, materials with C: 0.01 to 0.10 mass% can be used. However, steel plates with C: less than 0.01% are not excluded in the present invention. In addition, steel plates containing N, S, O, B, V, Nb, Ti, Cu, Mo, Cr, Co, Ni, Ca, Sr, In, Sn, Sb, etc. as trace additive elements in addition to C, Al, Si, Mn, and P also fall within the scope of the present invention.

[0087] In addition, there is no particular limitation on the method for obtaining the base steel sheet. For example, in the case of the hot-rolled steel sheet, a hot-rolled steel sheet that has been subjected to a hot rolling step and a pickling step may be used, and in the case of the cold-rolled steel sheet, a cold rolling step may be added for production. Furthermore, in order to obtain the characteristics of the steel sheet, a recrystallization annealing step may be performed before the hot-dip coating step.

[0088] Regarding the plating bath used when forming the above-mentioned plating film, as mentioned above, since the composition of the above-mentioned plating film as a whole is roughly the same as the composition of the plating bath, a plating bath with the following composition is used: containing 45 mass% to 65 mass% Al and 1.0 mass% to 3.0 mass% Si, and the remainder is essentially composed of Zn, Fe and unavoidable impurities.

[0089] The bath temperature of the plating bath is not particularly limited, but is preferably within a temperature range of (melting point + 20° C.) to 650° C.

[0090] The reason why the lower limit of the bath temperature of the coating bath is set to the melting point + 20°C is that in order to perform the melt coating treatment, the bath temperature needs to be above the solidification point, and by setting it to the melting point + 20°C, solidification caused by a local decrease in the bath temperature of the coating bath is prevented. On the other hand, the reason why the upper limit of the bath temperature is set to 650°C is that if it exceeds 650°C, it becomes difficult to quickly cool the coating film, and the interface alloy layer formed at the interface between the coating film and the base steel sheet may become thicker.

[0091] Furthermore, the temperature of the base steel sheet immersed in the coating bath (entry plate temperature) is not particularly limited. For example, from the perspective of ensuring coating characteristics in the continuous hot-dip coating operation or preventing bath temperature changes, it is preferably controlled within ±20°C relative to the temperature of the coating bath.

[0092] Furthermore, the time for immersing the base steel sheet in the coating bath is preferably 0.5 seconds or longer. The reason is that if the immersion time is less than 0.5 seconds, a sufficient coating film may not be formed on the surface of the base steel sheet. In addition, there is no particular upper limit to the immersion time, but if the immersion time is extended, the interface alloy layer formed between the coating film and the steel sheet may become thicker, so it is preferably set to within 8 seconds.

[0093] Furthermore, in the method for manufacturing a molten Al-Zn type plated steel sheet of the present invention, it is characterized in that, in the step of imparting the thermal history, the maximum temperature reached is above 150°C and below 277°C, the cooling time from the maximum temperature reached to 150°C is set to less than two hours, and the cooling time from 150°C to room temperature is set to more than three hours.

[0094] By providing such a thermal history, it is possible to obtain a molten Al—Zn-based plated steel sheet that is stable and excellent in bendability and corrosion resistance of the bent portion.

[0095] The reason for setting the maximum temperature reached when the thermal history is given to be 150°C or more and 277°C or less is that, when the maximum temperature reached is less than 150°C, the diffusion of Zn becomes slow, so that the solid solution strengthening and precipitation strengthening in the Al primary crystal cannot be fully eliminated, and the stripe-like structure in the Al-Zn eutectic also remains, so that the bending workability of the molten Al-Zn plated steel sheet cannot be fully obtained. On the other hand, if the maximum temperature reached exceeds 277°C, the solid solution strengthening and precipitation strengthening in the Al primary crystal are eliminated, and the stripe-like structure in the Al-Zn eutectic is also decomposed, but when it is cooled and passes 277°C, the stripe-like structure is generated again in the Al-Zn eutectic, resulting in poor bending workability of the molten Al-Zn plated steel sheet.

[0096] From the same viewpoint, the highest temperature reached when the thermal history is provided is preferably 170°C to 250°C, and more preferably 190°C to 230°C.

[0097] In addition, in the step of imparting the thermal history, the reason for setting the cooling time from the highest temperature reached to 150°C to less than two hours is that the growth of the interface alloy layer is suppressed, thereby achieving an improvement in bending workability. At the same time, the changes in the structure of the plated film reached in the heating stage during the cooling stage are suppressed as much as possible, thereby maintaining the elimination of the above-mentioned solid solution strengthening and precipitation strengthening, and suppressing the generation of striped structure.

[0098] From the same viewpoint, the cooling time from the highest reached temperature to 150° C. is preferably one hour or less.

[0099] Furthermore, in the step of imparting the thermal history, the cooling time from 150° C. to room temperature is set to three hours or more in order to ensure the temperature and time for the diffusion of Zn in the Al primary crystals, suppress the Zn content in the matrix to 30 mass % or less, make the maximum diameter of the Zn precipitates average to be 100 nm or more, and fully eliminate the solid solution strengthening and precipitation strengthening in the Al primary crystals. In addition, the "normal temperature" refers to room temperature, which is assumed to be about 25° C.

[0100] Furthermore, from the viewpoint of production efficiency, the cooling time from 150° C. to room temperature is preferably within ten hours.

[0101] Here, Figure 1 The equilibrium state diagram of the Al-Zn binary system is shown.

[0102] In a conventional melt-coating process, cooling after coating is rapid cooling, so Zn cannot be discharged from dendrites in time during solidification, and Zn is solidified in a state of being supersaturated (more than 30 mass%) in solid solution in the matrix. Therefore, Zn supersaturated in solid solution in the α-Al phase (matrix) of the primary Al crystal causes solid solution strengthening, and the hardness increases, resulting in a decrease in elongation and a decrease in bendability.

[0103] Furthermore, if heating is performed after the plating film is formed, the supersaturated Zn in the α-Al phase precipitates, the Zn solid solubility decreases, and in the subsequent cooling, the solidification is separated into the matrix of the α-Al phase and the Zn precipitates. At this time, it is known that by controlling the Zn content in the matrix to 30 mass % or less, the solid solution strengthening of the Al primary crystal is eliminated.

[0104] In addition, the Al-Zn eutectic is composed of an Al portion and a Zn portion. If it is heated to 277°C or higher, the Zn solid solubility of the Al portion increases, and the Zn portion is almost solid-dissolved, thereby becoming an Al portion that is more supersaturated with Zn. And it is known that by cooling after heating, it changes again to an Al-Zn eutectic below 277°C, and the Al-Zn eutectic becomes a striped structure in which the Al portion and the Zn portion are alternately arranged in stripes.

[0105] In addition, in the method for manufacturing a molten Al-Zn plated steel sheet of the present invention, steps other than the above-mentioned step of forming a coating film and the step of imparting a thermal history are not particularly limited, and any step can be appropriately implemented according to the performance required of the molten Al-Zn plated steel sheet.

[0106] In addition, the method may further include forming a coating film directly or via an intermediate layer on the molten Al-Zn based plated steel sheet obtained by the method for producing a molten Al-Zn based plated steel sheet of the present invention.

[0107] In addition, there is no particular limitation on the method for forming the coating film, and it can be appropriately selected according to the required performance. For example, a forming method such as roller coating, curtain coating, spray coating, etc. can be cited. After the coating containing the organic resin is applied, the coating film can be formed by heating and drying by hot air drying, infrared heating, induction heating, etc.

[0108] The intermediate layer is not particularly limited as long as it is a layer formed between the plated film of the hot-dip plated steel sheet and the coating film. The type or formation method of the intermediate layer is the same as that described in the hot-dip Al-Zn plated steel sheet of the present invention.

[0109] Example

[0110] <Samples 1 to 30>

[0111] (1) Production of molten Al-Zn plated steel sheets

[0112] A cold-rolled steel sheet with a thickness of 0.35 mm produced by a conventional method was used as a base steel sheet, and annealing and plating were performed using a continuous hot-dip plating device, thereby producing hot-dip Al-Zn-based plated steel sheets A to C having the plating film compositions and adhesion amounts shown in Table 1.

[0113] In addition, regarding the composition of the plating bath used in the manufacture of the hot-dip galvanized steel sheet, a composition based on Al: 55 mass%, Si: 1.6 mass%, Fe: 0.4 mass%, with the remainder essentially being Zn and unavoidable impurities (plating A) was used, and the composition in which the content of each component was changed was used (plating B, plating C).

[0114] In addition, the bath temperature of the coating bath was set to 590°C, and the plate temperature of the base steel plate was controlled to be the same as the coating bath temperature. Furthermore, the coating film adhesion was controlled to be 85±10 g / m on each side. 2 .

[0115] (2) Assignment of thermal history

[0116] The obtained molten Al—Zn-based plated steel sheets were subjected to thermal history under the conditions shown in Table 2 to obtain molten Al—Zn-based plated steel sheets of respective samples.

[0117] (3) Confirmation of the adhesion amount and composition of the plating film

[0118] A piece of 100 mm φ was punched out from the molten Al-Zn type plated steel sheet of each sample, and the non-measurement surface was sealed with tape. Then, as shown in JIS H 0401 (2013), the plated film was dissolved and peeled off using a mixed solution of hydrochloric acid and hexamethylenetetramine, and the adhesion amount of the plated film was calculated based on the mass difference of the sample before and after peeling.

[0119] Then, the stripping liquid was filtered, and the filtrate and the solid content were analyzed separately. Specifically, the filtrate was subjected to ICP emission spectrometry to quantify components other than insoluble Si.

[0120] Furthermore, the solid component was dried and ashed in a heating furnace at 650°C, and then melted by adding sodium carbonate and sodium tetraborate. In addition, the melt was dissolved with hydrochloric acid, and the insoluble Si was quantified by ICP emission spectrometry of the solution. The Si concentration in the plated film was obtained by adding the soluble Si concentration obtained by filtrate analysis and the insoluble Si concentration obtained by solid component analysis.

[0121] Table 1 shows the compositions and adhesion amounts of the obtained plated films A to C.

[0122]

Table 1

[0123]

[0124] <Evaluation>

[0125] The following evaluations were performed on each sample of the hot-dip Al-Zn-based plated steel sheet obtained as described above. The evaluation results are shown in Table 1.

[0126] (1) Conditions for coating film

[0127] The cross section of the plated film of each sample of the molten Al-Zn-based plated steel sheet was observed by ultra-low acceleration SEM and analyzed by energy dispersive X-ray spectroscopy (hereinafter referred to as "EDX").

[0128] The conditions for observation and analysis of the plated film were as follows: using ULTRA55 (ultra-low acceleration SEM) manufactured by Zeiss and Ultim Extreme (EDX) manufactured by Oxford Instruments, with an acceleration voltage of 3 kV and observation magnifications of 3,000 and 20,000 times, and spot analysis of predetermined locations.

[0129] In addition, the average value of the maximum diameter of the Zn-based precipitates existing in the Al primary crystals was obtained by observing three viewing fields at 20,000 times, extracting 10 points of Zn-based precipitates from the Al primary crystals in each viewing field in descending order, measuring their major diameters, and calculating the average. In addition, regarding the minimum period of the stripe-like structure, three viewing fields were observed at 20,000 times, the stripe period of the existing stripe-like structure was measured, and the smallest one among them was taken as the minimum period.

[0130] Table 2 shows the conditions of the obtained plating film (Zn concentration in the matrix and the average value of the maximum diameter of Zn precipitates, the presence or absence and the minimum period of the stripe structure of the Al—Zn eutectic, and the thickness of the interface alloy layer).

[0131] In addition, for the molten Al-Zn-based plated steel sheets of Samples 1 and 14, photographs obtained by observing precipitates mainly composed of Zn present in Al primary crystals are shown in FIG. Figure 2 .

[0132] Furthermore, for the molten Al-Zn-based plated steel sheets of Samples 1, 14, and 22, photographs obtained by observing the stripe structure of the Al-Zn eutectic are shown in FIG. Figure 3 .

[0133] (2) Bending workability

[0134] For each sample of the molten Al-Zn plated steel sheet, a bending test of "T bending" (bending test of the adhesion test of the coating according to JIS G3321 (2019)) was performed while reducing 2T in the range of 10T to 0T, and the limit of the bending T that became "crack-free" was confirmed when observed at 10 times with a magnifying glass. The results are shown in Table 2.

[0135] In addition, the so-called "T bend" is a 180° bend test performed while sandwiching the plate thickness of the steel plate. In addition, the so-called "no crack" during observation means that no crack is observed at all when the outer front end of the bent portion is observed at 10 times using a magnifying glass. And the so-called "bend T limit" refers to the smallest T among the T bends without cracks. For example, when no cracks are observed in the 6T bend and cracks are observed in the 4T bend, the bend T limit is "6T".

[0136] (3) Corrosion resistance of the bent part

[0137] The molten Al-Zn plated steel sheets of Sample 1 and Sample 14 were subjected to outdoor exposure tests in the Chuo-ku, Chiba City, while being T-bent in the range of 0T to 9T. The bent portions after the 4-year and 8-month exposure tests were visually observed and evaluated according to the following criteria. The evaluation results are shown in Figure 4 .

[0138] (Evaluation Criteria)

[0139] One point: Red rust is clearly present

[0140] Second point: Slight red rust

[0141] Three points: no red rust

[0142]

[0143] According to Table 2 and Figure 4 As a result, it can be seen that each sample of the present invention example has a well-balanced and excellent bending workability and corrosion resistance of the processed portion compared with each sample of the comparative example.

[0144] Industrial Applicability

[0145] According to the present invention, it is possible to provide a hot-dip Al—Zn-based plated steel sheet having stable bending workability and excellent corrosion resistance of a bent portion, and a method for producing the same.

Claims

1. A molten Al-Zn plated steel sheet, characterized in that: The invention relates to a steel sheet having a plated film and an interface alloy layer, wherein the plated film has the following composition: contains 45 mass % to 65 mass % of Al and 1.0 mass % to 3.0 mass % of Si, and the remainder is composed of Zn, Fe and inevitable impurities, and the interface alloy layer is formed on the interface side between the plated film and the base steel sheet, and contains Fe, Al, Si, Zn and inevitable impurities, The plated film has dendrites mainly composed of Al primary crystals and interdendritic gaps containing Al-Zn eutectics. The Al primary crystals include a matrix of an α-Al phase and Zn precipitates, and the Zn content in the matrix is ​​30 mass % or less. The thickness of the interface alloy layer is less than 1 μm.

2. The molten Al-Zn based plated steel sheet according to claim 1, characterized in that: The average value of the maximum diameter of the Zn precipitates in the Al primary crystals is 100 nm or more.

3. The molten Al-Zn based plated steel sheet according to claim 1 or 2, characterized in that: The Al—Zn eutectic in the interdendritic gap does not have a striped structure with a period of less than 2 μm.

4. A method for producing a molten Al-Zn based plated steel sheet, which is the method for producing a molten Al-Zn based plated steel sheet according to claim 1 or 2, characterized in that: include: A step of forming a plating film on a base steel sheet, wherein the plating film has a composition comprising 45 mass % to 65 mass % of Al and 1.0 mass % to 3.0 mass % of Si, with the remainder being Zn, Fe and inevitable impurities; and After forming the plating film, a step of providing the steel sheet with a thermal history having a maximum temperature of 150° C. to 277° C., In the step of imparting the thermal history, the cooling time from the highest reached temperature to 150° C. is set to less than two hours, and the cooling time from 150° C. to room temperature is set to more than three hours.