Mask capable of being torn and pulled and preparation method thereof

By combining polyurethane and polyvinyl alcohol, combined with trehalose, carnosine, triethanolamine and other ingredients, a painless and tear-free rasp-able mask can be prepared without water, which solves the problem of pricking the existing mask during tearing and pulling. Pain and the need to moisturize with water improves moisturizing and permeability.

CN119033597APending Publication Date: 2024-11-29SHENGYUAN (GUANGZHOU) BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213857.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing tear-able masks are prone to stinging the skin during tearing and need to be moistened with water before they can be completely removed. The amount of film-forming agents is large or uneven, which affects the user experience.

Method used

By combining polyurethane and polyvinyl alcohol, combined with trehalose, carnosine, triethanolamine and other ingredients, the A and B components are formed, and the mask is prepared by using specific stirring and cooling steps to ensure that the mask is painless when tearing and does not require water. Can be torn off completely.

Benefits of technology

It achieves a painless tearing effect, enhances the moisturizing and permeability of the mask, and reduces the use of film-forming agents, improving the stability and skin comfort of the mask.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020957770000071
    Figure BDA0005020957770000071
  • Figure BDA0005020957770000081
    Figure BDA0005020957770000081
  • Figure BDA0005020957770000082
    Figure BDA0005020957770000082
Patent Text Reader

Abstract

The invention relates to a tearable mask and a preparation method thereof, and belongs to the technical field of skin care products. The tearable facial mask comprises a component A and a component B, the component A is prepared from the following components in parts by mass: 10 to 15 parts of polyvinyl alcohol, 0.1 to 0.5 part of trehalose, 0.01 to 0.05 part of first preservative, 0.1 to 0.5 part of chelating agent and 100 parts of water; the component B is prepared from the following components in parts by mass: 1 to 3 parts of polyurethane, 0.1 to 0.5 part of carnosine, 0.1 to 0.5 part of triethanolamine, 0.01 to 0.05 part of second preservative, 0.1 to 0.5 part of aromatic and 0.1 to 3 parts of thickening agent. The tearable facial mask can effectively improve the moisturizing effect of the skin, and the active ingredients of the tearable facial mask can be well absorbed by the skin in the using process; on the other hand, the tearable mask can be completely torn and removed from the surface of the skin, and no pain is caused.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of skin care products, and in particular relates to a tearable facial mask and a preparation method thereof. Background Art

[0002] A peelable mask is a mask that is made by evenly applying a liquid in the form of a lotion, paste or spray to the face, and then peeling off the film after it dries. A peelable mask needs to be able to form a continuous film in a short time and not break during the tearing process, which requires the film to have good elasticity and tensile strength, and moderate adhesion between the film and the skin.

[0003] In order to ensure that the tearable mask can form a continuous film on the skin surface in a short time and the film does not break during the tearing process, the film-forming agent in the tearable mask is an extremely important component. When polyvinyl alcohol or polyvinyl pyrrolidone film-forming agents are used, the skin will have a very strong sense of pain during the tearing process of the film due to the strong adhesion of such film-forming agents to the skin. When acrylic film-forming agents are used, since such film-forming agents are too hard and easy to break, the film cannot be completely torn off the skin regardless of whether it is wetted with water. When polyurethane film-forming agents are used, the film can be completely torn off from the skin after wetting. Since the polyurethane film-forming agent has good elasticity, the mask can be completely torn off from the skin surface after re-wetting with water, but the mask needs to be applied to the skin in large quantities to cover the color of the skin itself, or more polyurethane film-forming agents need to be added to the mask to achieve this.

[0004] It can be seen that developing a tearable mask that can be completely torn off from the skin surface without wetting with water and without pain is still an urgent problem to be solved. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a tearable facial mask and a preparation method thereof, which utilizes the moisturizing and film-forming properties of polyurethane and is compounded with polyvinyl alcohol to achieve a good moisturizing effect without irritating the skin and causing pain.

[0006] The first object of the present invention is to provide a tearable facial mask, comprising component A and component B;

[0007] The component A comprises, by mass, 10-15 parts of polyvinyl alcohol, 0.1-0.5 parts of trehalose, 0.01-0.05 parts of a first preservative, 0.1-0.5 parts of a chelating agent and 100 parts of water;

[0008] The B component includes, by mass, 1-3 parts of polyurethane, 0.1-0.5 parts of carnosine, 0.1-0.5 parts of triethanolamine, 0.01-0.05 parts of a second preservative, 0.1-0.5 parts of a fragrance, and 0.1-3 parts of a thickener.

[0009] In one embodiment of the present invention, the first preservative is p-hydroxyacetophenone.

[0010] In one embodiment of the present invention, the chelating agent is disodium ethylenediaminetetraacetate.

[0011] In one embodiment of the present invention, the polyurethane is polyurethane-35.

[0012] In one embodiment of the present invention, the second preservative is phenoxyethanol.

[0013] In one embodiment of the present invention, the fragrance is essence.

[0014] In one embodiment of the present invention, the thickener is selected from one or more of xanthan gum, carrageenan, hydroxyethyl cellulose and polyvinyl alcohol.

[0015] The second object of the present invention is to provide a method for preparing the tearable facial mask, comprising the following steps:

[0016] S1, adding polyvinyl alcohol, trehalose, a first preservative, and a chelating agent into water, stirring and heating, to obtain component A;

[0017] S2. Cooling the component A described in S1, sequentially adding polyurethane, carnosine, triethanolamine, a second preservative, a fragrance and a thickener, stirring evenly, to obtain the tearable facial mask.

[0018] In one embodiment of the present invention, in S1, the stirring and heating temperature is 80°C-90°C, and the time is 15min-25min; polyvinyl alcohol needs to be completely dissolved to no particles under this condition, otherwise it will affect the film-forming properties of the tearable mask.

[0019] In one embodiment of the present invention, in S2, the cooling is to 35°C-45°C; when adding polyurethane, it must be added at a low temperature, otherwise the material will agglomerate, affecting the efficacy of the tearable mask.

[0020] The technical solution of the present invention has the following advantages over the prior art:

[0021] (1) The polyurethane used in the tearable mask of the present invention has good elasticity and ductility, and can provide unparalleled skin-fitting and comfort; in addition, polyurethane also has excellent moisturizing properties, and can effectively lock in moisture, keeping the skin moist and soft. The tearable mask compounded with polyvinyl alcohol and polyurethane is white when applied on the face, transparent and colorless after drying, and there is no stinging sensation when it is torn off.

[0022] (2) The tearable mask of the present invention comprises component A and component B, and the raw materials of each phase in the formula cooperate with each other, so that the prepared tearable mask has good moisture retention and painless tearing performance. Trehalose in component A and chelating agent disodium ethylenediaminetetraacetic acid are compatible with each other, so that after the tearable mask is applied to the skin, a protective film is formed on the cell surface layer, which maintains the original nutrition and moisture of the skin and nourishes the skin cells, thereby enhancing the water-locking and moisture-keeping ability of the tearable mask. The carnosine in component B synergistically enhances the water absorption capacity of the outermost layer of the skin and improves the water-locking and moisture-keeping property of the tearable mask. At the same time, it promotes the penetration of nutrients in the tearable mask into human skin and improves the skin permeability of the tearable mask. Carnosine and triethanolamine are compatible with each other, which enhances the dispersibility of each raw material in the tearable mask, so that each raw material in the tearable mask formula is dispersed more evenly and improves the stability of the tearable mask. By combining p-hydroxyacetophenone in component A and phenoxyethanol in component B, the antiseptic effect of the peelable mask can be effectively improved.

[0023] (3) The tearable facial mask of the present invention can effectively improve the moisturizing effect of the skin and the active ingredients of the tearable facial mask can be better absorbed by the skin during use; on the other hand, the tearable facial mask can be completely torn off from the skin surface without pain. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. It should be understood that the specific embodiments are only used to explain the present invention, but the embodiments are not intended to limit the present invention.

[0025] In the present invention, unless otherwise explained, technical and scientific terms used in the present invention have the same meanings as commonly understood by those skilled in the art to which the present invention belongs.

[0026] In the present invention, unless otherwise stated, the term "and / or" used in the present invention includes any and all combinations of one or more of the associated listed items.

[0027] In the present invention, unless otherwise stated, the experimental methods used in the embodiments of the present invention are conventional methods unless otherwise stated, and the materials, reagents, etc. used are all commercially available unless otherwise stated.

[0028] Example 1

[0029] The tearable mask of this embodiment includes component A and component B, and the original composition and mass fraction of each component are as follows:

[0030] Component A includes, by mass, 12 parts of polyvinyl alcohol, 0.3 parts of trehalose, 0.03 parts of preservative p-hydroxyacetophenone, 0.3 parts of chelating agent disodium ethylenediaminetetraacetate, and 100 parts of water;

[0031] Component B includes, by mass, 352 parts of polyurethane, 0.3 parts of carnosine, 0.3 parts of triethanolamine, 0.03 parts of preservative phenoxyethanol, 0.3 parts of fragrance essence, and 1 part of thickener hydroxyethyl cellulose.

[0032] The specific steps include:

[0033] S1. Add polyvinyl alcohol, trehalose, preservative p-hydroxyacetophenone, chelating agent disodium ethylenediaminetetraacetate and water into a vacuum emulsifying pot, heat to 85°C until the materials are completely dissolved, and keep the temperature constant for 20 minutes to obtain component A;

[0034] S2. Cool component A to 40°C, add polyurethane-35, carnosine, triethanolamine, preservative phenoxyethanol, fragrance essence and thickener hydroxyethyl cellulose in sequence, stir evenly, and obtain a tearable facial mask.

[0035] Example 2

[0036] The tearable mask of this embodiment includes component A and component B, and the original composition and mass fraction of each component are as follows:

[0037] Component A includes, by mass, 10 parts of polyvinyl alcohol, 0.1 parts of trehalose, 0.01 parts of preservative p-hydroxyacetophenone, 0.1 parts of chelating agent disodium ethylenediaminetetraacetate, and 100 parts of water;

[0038] Component B includes, by mass, 1 part of polyurethane-35, 0.1 part of carnosine, 0.1 part of triethanolamine, 0.01 part of preservative phenoxyethanol, 0.1 part of fragrance essence, and 0.1 part of thickener hydroxyethyl cellulose.

[0039] The specific steps include:

[0040] S1. Add polyvinyl alcohol, trehalose, preservative p-hydroxyacetophenone, chelating agent disodium ethylenediaminetetraacetate and water into a vacuum emulsifying pot, heat to 80°C until the materials are completely dissolved, and keep the temperature constant for 25 minutes to obtain component A;

[0041] S2. Cool component A to 35°C, add polyurethane-35, carnosine, triethanolamine, preservative phenoxyethanol, fragrance essence and thickener hydroxyethyl cellulose in sequence, stir evenly, and obtain a tearable facial mask.

[0042] Example 3

[0043] The tearable mask of this embodiment includes component A and component B, and the original composition and mass fraction of each component are as follows:

[0044] Component A includes, by mass, 15 parts of polyvinyl alcohol, 0.5 parts of trehalose, 0.05 parts of preservative p-hydroxyacetophenone, 0.5 parts of chelating agent disodium ethylenediaminetetraacetate, and 100 parts of water;

[0045] Component B includes, by mass, 353 parts of polyurethane, 0.5 parts of carnosine, 0.5 parts of triethanolamine, 0.05 parts of preservative phenoxyethanol, 0.5 parts of fragrance essence, and 2 parts of thickener hydroxyethyl cellulose.

[0046] The specific steps include:

[0047] S1. Add polyvinyl alcohol, trehalose, preservative p-hydroxyacetophenone, chelating agent disodium ethylenediaminetetraacetate and water into a vacuum emulsifying pot, raise the temperature to 90° C. until the materials are completely dissolved, and keep the temperature constant for 15 minutes to obtain component A;

[0048] S2. Cool component A to 45°C, add polyurethane-35, carnosine, triethanolamine, preservative phenoxyethanol, fragrance essence and thickener hydroxyethyl cellulose in sequence, stir evenly, and obtain a tearable facial mask.

[0049] Comparative Example 1

[0050] The peelable facial mask of this comparative example includes component A and component B, and the original composition and mass fraction of each component are as follows:

[0051] Component A includes, by mass, 12 parts of polyvinyl alcohol, 0.3 parts of trehalose, 0.03 parts of preservative p-hydroxyacetophenone, 0.3 parts of chelating agent disodium ethylenediaminetetraacetate, and 100 parts of water;

[0052] Component B includes, by mass, 2 parts of VP / VA copolymer, 0.3 parts of carnosine, 0.3 parts of triethanolamine, 0.03 parts of preservative phenoxyethanol, 0.3 parts of fragrance essence, and 1 part of thickener hydroxyethyl cellulose.

[0053] The specific steps include:

[0054] S1. Add polyvinyl alcohol, trehalose, preservative p-hydroxyacetophenone, chelating agent disodium ethylenediaminetetraacetate and water into a vacuum emulsifying pot, heat to 85°C until the materials are completely dissolved, and keep the temperature constant for 20 minutes to obtain component A;

[0055] S2. Cool component A to 40°C, add VP / VA copolymer, carnosine, triethanolamine, preservative phenoxyethanol, fragrance essence and thickener hydroxyethyl cellulose in sequence, stir evenly, and obtain a tearable facial mask.

[0056] Comparative Example 2

[0057] The peelable facial mask of this comparative example includes component A and component B, and the original composition and mass fraction of each component are as follows:

[0058] Component A includes, by mass, 12 parts of polyvinyl alcohol, 0.3 parts of trehalose, 0.03 parts of preservative p-hydroxyacetophenone, 0.3 parts of chelating agent disodium ethylenediaminetetraacetate, and 100 parts of water;

[0059] Component B includes, by mass, 0.3 parts of carnosine, 0.3 parts of triethanolamine, 0.03 parts of preservative phenoxyethanol, 0.3 parts of fragrance essence, and 1 part of thickener hydroxyethyl cellulose.

[0060] The specific steps include:

[0061] S1. Add polyvinyl alcohol, trehalose, preservative p-hydroxyacetophenone, chelating agent disodium ethylenediaminetetraacetate and water into a vacuum emulsifying pot, heat to 85°C until the materials are completely dissolved, and keep the temperature constant for 20 minutes to obtain component A;

[0062] S2. Cool component A to 40° C., add carnosine, triethanolamine, preservative phenoxyethanol, fragrance essence and thickener hydroxyethyl cellulose in sequence, stir evenly, and obtain a tearable facial mask.

[0063] Comparative Example 3

[0064] The peelable facial mask of this comparative example includes component A and component B, and the original composition and mass fraction of each component are as follows:

[0065] Component A includes, by mass, 12 parts of polyvinyl alcohol, 0.03 parts of preservative p-hydroxyacetophenone, 0.3 parts of chelating agent disodium ethylenediaminetetraacetate, and 100 parts of water;

[0066] Component B includes, by mass, 352 parts of polyurethane, 0.3 parts of carnosine, 0.3 parts of triethanolamine, 0.03 parts of preservative phenoxyethanol, 0.3 parts of fragrance essence, and 1 part of thickener hydroxyethyl cellulose.

[0067] The specific steps include:

[0068] S1. Add polyvinyl alcohol, preservative p-hydroxyacetophenone, chelating agent disodium ethylenediaminetetraacetate and water into a vacuum emulsifying pot, raise the temperature to 85°C until the materials are completely dissolved, and keep the temperature constant for 20 minutes to obtain component A;

[0069] S2. Cool component A to 40°C, add polyurethane-35, carnosine, triethanolamine, preservative phenoxyethanol, fragrance essence and thickener hydroxyethyl cellulose in sequence, stir evenly, and obtain a tearable facial mask.

[0070] Comparative Example 4

[0071] The peelable facial mask of this comparative example includes component A and component B, and the original composition and mass fraction of each component are as follows:

[0072] Component A includes, by mass, 12 parts of polyvinyl alcohol, 0.3 parts of trehalose, 0.03 parts of preservative p-hydroxyacetophenone, 0.3 parts of chelating agent disodium ethylenediaminetetraacetate, and 100 parts of water;

[0073] Component B includes, by mass, 352 parts of polyurethane, 0.3 parts of carnosine, 0.03 parts of preservative phenoxyethanol, 0.3 parts of fragrance essence, and 1 part of thickener hydroxyethyl cellulose.

[0074] The specific steps include:

[0075] S1. Add polyvinyl alcohol, trehalose, preservative p-hydroxyacetophenone, chelating agent disodium ethylenediaminetetraacetate and water into a vacuum emulsifying pot, heat to 85°C until the materials are completely dissolved, and keep the temperature constant for 20 minutes to obtain component A;

[0076] S2. Cool component A to 40°C, add polyurethane-35, carnosine, preservative phenoxyethanol, fragrance essence and thickener hydroxyethyl cellulose in sequence, stir evenly to obtain a tearable facial mask.

[0077] Test Example 1

[0078] The moisturizing effect of the tearable facial masks of Examples 1-3 and Comparative Examples 1-4 was tested by drawing a 3×3 cm 2 The left arm was used as the test area for moisturizing products, and the corresponding symmetrical area on the right arm was used as the blank control. Then, Corneometer CM825 was used to test the change in the capacitance value of the stratum corneum of each test site before and after using the product to measure the change in the stratum corneum water content. This was repeated 5 times to obtain the average value. The hydration rate of the stratum corneum of the skin = (test value - blank value) / blank value × 100%. The hydration rate test results are shown in Table 1:

[0079] Table 1

[0080]

[0081]

[0082] It can be seen from Table 1 above that in terms of moisturizing, the facial masks of Examples 1-4 have excellent moisturizing effects.

[0083] Test Example 2

[0084] The use effects of the peelable facial masks of Examples 1-3 and Comparative Examples 1-4 were tested, with 10 people forming a judging panel, a total of 7 groups, and the blind test scores were averaged; 1 point was the worst and 5 points were the best.

[0085] Film-forming property: Apply the tear-off mask to the face and back of the hand respectively. After it dries and becomes transparent after 30 minutes, gently peel it off to observe whether the tear-off mask can be peeled off in a gauze-like state and whether there is any cracking.

[0086] Extensibility: Apply the tear-off mask to the face and back of the hand respectively. After it dries and becomes transparent after 30 minutes, observe whether a continuous film can be formed and whether there is uneven distribution.

[0087] Fit: Apply the tear-off mask to the face and back of the hand respectively. After it dries and becomes transparent after 30 minutes, observe whether the transparent film is completely fitted to the skin.

[0088] Firming: Apply the peelable mask to the face and back of the hands respectively. After 30 minutes of drying and becoming transparent, feel the firming feeling of the peelable mask on the skin.

[0089] Breathability: Apply the peelable mask to the face and back of the hand respectively. After 30 minutes of drying and becoming transparent, feel whether the peelable mask feels sticky or airtight on the skin.

[0090] Pain: Apply the peelable mask to the face and back of the hands respectively. After it dries and becomes transparent after 30 minutes, gently peel it off and feel whether the skin feels any pain.

[0091] The relevant evaluation results are shown in Table 2:

[0092] Table 2

[0093]

[0094]

[0095] As can be seen from Table 2, the tearable mask of the embodiment of the present invention can be evenly applied to the skin when used, can completely fit the skin of the face and the back of the hands, is breathable and not tight after film formation, and has the effect of tightening the skin at the same time; when the film is torn off from the skin surface, it is not necessary to wet the film in advance, and the mask can be completely torn off from the skin surface without any tearing pain.

[0096] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A tearable facial mask, characterized in that: It includes component A and component B; The component A comprises, by mass, 10-15 parts of polyvinyl alcohol, 0.1-0.5 parts of trehalose, 0.01-0.05 parts of a first preservative, 0.1-0.5 parts of a chelating agent and 100 parts of water; The B component includes, by mass, 1-3 parts of polyurethane, 0.1-0.5 parts of carnosine, 0.1-0.5 parts of triethanolamine, 0.01-0.05 parts of a second preservative, 0.1-0.5 parts of a fragrance, and 0.1-3 parts of a thickener.

2. The tearable facial mask according to claim 1, characterized in that: The first preservative is p-hydroxyacetophenone.

3. The tearable facial mask according to claim 1, characterized in that: The chelating agent is disodium ethylenediaminetetraacetate.

4. The tearable facial mask according to claim 1, characterized in that: The polyurethane is polyurethane-35.

5. The tearable facial mask according to claim 1, characterized in that: The second preservative is phenoxyethanol.

6. The tearable facial mask according to claim 1, characterized in that: The aromatic agent is essence.

7. The tearable facial mask according to claim 1, characterized in that: The thickener is selected from one or more of xanthan gum, carrageenan, hydroxyethyl cellulose and polyvinyl alcohol.

8. A method for preparing a tearable facial mask according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, adding polyvinyl alcohol, trehalose, a first preservative, and a chelating agent into water, stirring and heating, to obtain component A; S2. Cooling the component A described in S1, adding polyurethane, carnosine, triethanolamine, a second preservative, a fragrance and a thickener in sequence, stirring evenly, and obtaining the tearable facial mask.

9. The method for preparing the tearable facial mask according to claim 8, characterized in that: In S1, the stirring and heating temperature is 80°C-90°C, and the time is 15min-25min.

10. The method for preparing the tearable facial mask according to claim 8, characterized in that: In S2, the temperature is lowered to 35°C-45°C.