Efficient in-furnace deacidification agent and preparation method thereof

By adsorbing baking soda solution into the pores of diatomaceous earth and burying it in calcium carbonate particles, an efficient deacidant was prepared, which solved the problems of low efficiency and high cost of traditional deacidant in the high temperature environment in the furnace, and achieved efficient deacidation Acid and heavy metal reduction effect.

CN119034467APending Publication Date: 2024-11-29JIANGSU KEHUI ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411157178.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The traditional waste incineration flue gas deacidification method relies on the rear-channel deacidification tower, which is difficult to meet strict environmental protection standards. In addition, the traditional furnace deacidifier is prone to agglomeration and agglomeration in high temperature environments, resulting in low deacidification efficiency and high cost.

Method used

Adsorb the baking soda solution into the pores of diatomaceous earth and is embedded in calcium carbonate particles to prepare high-efficiency deacidant. By vacuum drying and crushing at low temperature, deacidant particles with high specific surface area are formed to ensure high temperature in the furnace. Effective decomposition and expansion in the environment to improve the deacidification efficiency.

Benefits of technology

It significantly improves the deacidification efficiency, reduces the deacidification cost, avoids the agglomeration and agglomeration problems of traditional deacidants, and reduces the heavy metal ion content through phosphate buffers, saving fly ash treatment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an efficient in-furnace deacidification agent and a preparation method thereof. The efficient in-furnace deacidification agent is prepared from the following raw materials in parts by weight: 20-40 parts of diatomite, 50-80 parts of calcium carbonate, 20-30 parts of baking soda, 10-15 parts of a buffering agent, 3-5 parts of a dispersing agent and 80-120 parts of water. The preparation method of the in-furnace deacidification agent disclosed by the invention comprises the following steps: dissolving and depositing the baking soda in the pores of the diatomite, and then wrapping the surface of the diatomite with the calcium carbonate to obtain the in-furnace deacidification agent. According to the in-furnace deacidification agent disclosed by the invention, baking soda is quickly decomposed and expanded after the in-furnace deacidification agent encounters high temperature, surface calcium carbonate is exploded, and the in-furnace deacidification agent has the advantages of high deacidification efficiency, coking resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of waste incineration flue gas deacidification, and in particular to a high-efficiency in-furnace deacidification agent and a preparation method thereof. Background Art

[0002] Waste incineration flue gas deacidification is an essential part of the waste incineration power generation process. It aims to remove acid gases such as hydrogen chloride (HCl), sulfur dioxide (SO2), and hydrogen fluoride (HF) contained in the flue gas generated by waste incineration, so that the acid gas content in the flue gas reaches the national or local emission standards. At present, waste incineration deacidification is mainly carried out through the post-acidification tower, but with the increasingly stringent environmental protection standards, it is difficult to meet the new standards by relying solely on the deacidification tower to reduce the acid content in the flue gas. Most power plants rely on increasing the amount of traditional deacidification agents to lower other acid emission indicators. Not only is the effect not obvious, but it will also greatly increase the cost of deacidification, which has become a technical pain point in the industry.

[0003] Deacidification in the incineration stage, that is, adding deacidifiers in the incinerator, can not only reduce the amount of acid gas volatilization from the source, but also reduce the deacidification cost of the deacidification tower. It is a measure that kills two birds with one stone. At present, in areas with strict environmental protection policies or concentrated industrial waste, attempts have been made to use this method to reduce flue gas indicators. However, the deacidification environment in the furnace and the deacidification tower is very different. Traditional deacidifiers such as slaked lime and baking soda, if used directly in the furnace, will have low deacidification efficiency and serious ash accumulation due to the high flue gas flow rate and insufficient contact reaction between the deacidifier and the flue gas. Therefore, there is an urgent need to develop a targeted denitrification agent for the furnace. The present application prepares a high-efficiency deacidifying agent by adsorbing a baking soda solution into the pores of diatomaceous earth and then embedding the whole solution in calcium carbonate particles. When exposed to high temperature in a furnace, the baking soda decomposes and expands to "explode" the surface calcium carbonate, thus overcoming the agglomeration and caking problems of traditional deacidifying agents and greatly improving the deacidification efficiency. Summary of the invention

[0004] To achieve the above object, the present invention provides the following technical solutions: A highly efficient in-furnace deacidifying agent and a preparation method thereof, characterized in that the raw materials of the deacidifying agent include (by weight): 20-40 parts of diatomaceous earth, 50-80 parts of calcium carbonate, 20-30 parts of baking soda, 10-15 parts of buffer, 3-5 parts of dispersant, and 80-120 parts of water.

[0005] Furthermore, the preparation process comprises the following steps: (1) Add baking soda to water and fully dissolve it to prepare a baking soda solution; (2) adding diatomaceous earth to the baking soda solution prepared in step (1), and slowly stirring until a viscous liquid is obtained; (3) Add the viscous liquid obtained in step (2) into a blender, then add a dispersant, calcium carbonate, and a buffer, and stir for 15-30 minutes to obtain a premix; (4) removing the internal moisture of the premix prepared in step (3) by low-temperature vacuum drying to obtain a block deacidifying agent; (5) adding the block deacidifying agent obtained in step (4) into a crusher for crushing to obtain deacidifying agent particles; (6) Add the deacidifying agent particles obtained in step (5) into a pulverizer for crushing, grinding, and sieving to obtain a deacidifying agent finished product.

[0006] Furthermore, the diatomaceous earth particle size is 30-100 μm; Furthermore, the calcium carbonate is light calcium carbonate with a particle size of 1-5 μm; Further, the buffer is one or more of sodium pyrophosphate, sodium hexametaphosphate, and sodium tripolyphosphate; Furthermore, the dispersant is a polymer dispersant, specifically one or more of polycarboxylate, maleic anhydride copolymer, and polyacrylic acid; Furthermore, in the preparation step (4), the drying process parameters are vacuum degree 5-10 kPa, drying temperature 50-80° C., and drying time 60-90 min; Furthermore, the sieve used in the preparation step (6) is 300-500 mesh.

[0007] Due to the adoption of the above technical solution, this application has the following significant advantages: 1. The present invention absorbs baking soda into the pores of diatomite in an ionic state, and then embeds it in calcium carbonate particles to prepare a high-efficiency furnace deacidification agent. Baking soda is rapidly decomposed in a high temperature (200-300°C) environment in the furnace to produce carbon dioxide and water vapor. The expansion of carbon dioxide gas will "blow up" the surface calcium carbonate and produce a large number of pores, which greatly increases the overall specific surface area of ​​the deacidification agent, overcomes the problem of easy agglomeration and agglomeration of traditional calcium carbonate, and significantly improves the deacidification efficiency; 2. The present application adds a phosphate buffer in the process of preparing the deacidifying agent, which not only improves the dispersion uniformity of the calcium carbonate particles, but also reacts with the free heavy metals in the garbage, such as lead and chromium, to produce stable heavy metal salts, which helps to reduce the heavy metal ion content in the fly ash of garbage incineration and save the cost of fly ash treatment; 3. The present application adopts low-temperature vacuum drying in the preparation process of the deacidifying agent, which is conducive to the full and rapid volatilization of water in the powder. The bonding strength between the calcium carbonate particles after drying is low, and it is easy to crush and not easy to agglomerate in subsequent processing. It has a larger specific surface area and higher deacidification efficiency. BRIEF DESCRIPTION OF THE DRAWINGS In order to better illustrate the beneficial effects of the present invention, the accompanying drawings are briefly described as follows: Figure 1 is a process flow chart of the present invention, and performance testing of samples in embodiments of the present invention is performed; Figure 2 is a test device for testing sample specific surface area (BET), particle size (D50) and deacidification efficiency. DETAILED DESCRIPTION

[0008] The technical solutions in the embodiments of the present invention are described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0009] (1) Add 20 parts of baking soda to 80 parts of water and fully dissolve to prepare a baking soda solution; (2) Add 20 parts of diatomaceous earth to the baking soda solution and stir slowly until it becomes a viscous liquid; (3) Add the liquid from step (2) into a mortar mixer, then add 3 parts of dispersant, 50 parts of calcium carbonate, and 10 parts of buffer, and stir for 15 minutes to obtain a premix; (4) The premix is ​​dried under low temperature vacuum at a vacuum degree of 5 kPa, a drying temperature of 50 °C, and a drying time of 60 min to remove the internal moisture and obtain a block deacidifying agent; (5) Adding the block deacidifying agent into a crusher for crushing to obtain deacidifying agent particles; (6) The deacidifying agent particles are added to a pulverizer for crushing, grinding, and sieving to obtain a finished deacidifying agent product. Example

[0010] (1) Add 25 parts of baking soda to 85 parts of water and fully dissolve to prepare a baking soda solution; (2) Add 23 parts of diatomaceous earth to the baking soda solution and stir slowly until it becomes a viscous liquid; (3) Add the liquid from step (2) into a mortar mixer, then add 4 parts of dispersant, 70 parts of calcium carbonate, and 12 parts of buffer, and stir for 15 minutes to obtain a premix; (4) The premix is ​​dried under low temperature vacuum at a vacuum degree of 6 kPa, a drying temperature of 60 °C, and a drying time of 6 min to remove the internal moisture and obtain a block deacidifying agent; (5) Adding the block deacidifying agent into a crusher for crushing to obtain deacidifying agent particles; (6) The deacidifying agent particles are added to a pulverizer for crushing, grinding, and sieving to obtain a finished deacidifying agent product. Example

[0011] (1) Add 24 parts of baking soda to 90 parts of water and fully dissolve to prepare a baking soda solution; (2) Add 20 parts of diatomaceous earth to the baking soda solution and stir slowly until it becomes a viscous liquid; (3) Add the liquid from step (2) into a mortar mixer, then add 4 parts of dispersant, 60 parts of calcium carbonate, and 13 parts of buffer, and stir for 18 minutes to obtain a premix; (4) The premix is ​​dried by low-temperature vacuum drying at a vacuum degree of 7 kPa, a drying temperature of 70 °C, and a drying time of 70 min to remove the internal moisture and obtain a block deacidifying agent; (5) Adding the block deacidifying agent into a crusher for crushing to obtain deacidifying agent particles; (6) The deacidifying agent particles are added to a pulverizer for crushing, grinding, and sieving to obtain a finished deacidifying agent product. Example

[0012] (1) Add 25 parts of baking soda to 90 parts of water and fully dissolve to prepare a baking soda solution; (2) Add 30 parts of diatomaceous earth to the baking soda solution and stir slowly until it becomes a viscous liquid; (3) Add the liquid from step (2) into a mortar mixer, then add 4 parts of dispersant, 57 parts of calcium carbonate, and 15 parts of buffer, and stir for 20 minutes to obtain a premix; (4) The premix is ​​dried by low-temperature vacuum drying at a vacuum degree of 8 kPa, a drying temperature of 50 °C, and a drying time of 90 min to remove the internal moisture and obtain a block deacidifying agent; (5) Adding the block deacidifying agent into a crusher for crushing to obtain deacidifying agent particles; (6) The deacidifying agent particles are added to a pulverizer for crushing, grinding, and sieving to obtain a finished deacidifying agent product. Example

[0013] (1) Add 20 parts of baking soda to 100 parts of water and fully dissolve to prepare a baking soda solution; (2) Add 32 parts of diatomaceous earth to the baking soda solution and stir slowly until it becomes a viscous liquid; (3) Add the liquid from step (2) into a mortar mixer, then add 5 parts of dispersant, 80 parts of calcium carbonate, and 15 parts of buffer, and stir for 30 minutes to obtain a premix; (4) The premix is ​​dried under low temperature vacuum at a vacuum degree of 9 kPa, a drying temperature of 70°C, and a drying time of 80 min to remove the internal moisture and obtain a block deacidifying agent; (5) Adding the block deacidifying agent into a crusher for crushing to obtain deacidifying agent particles; (6) The deacidifying agent particles are added to a pulverizer for crushing, grinding, and sieving to obtain a finished deacidifying agent product. Example

[0014] (1) Add 25 parts of baking soda to 110 parts of water and fully dissolve to prepare a baking soda solution; (2) Add 35 parts of diatomaceous earth to the baking soda solution and stir slowly until it becomes a viscous liquid; (3) Add the liquid from step (2) into a mortar mixer, then add 5 parts of dispersant, 75 parts of calcium carbonate, and 14 parts of buffer, and stir for 18 minutes to obtain a premix; (4) The premix is ​​dried by low-temperature vacuum drying at a vacuum degree of 10 kPa, a drying temperature of 80° C., and a drying time of 80 min to remove the internal moisture and obtain a block deacidifying agent; (5) Adding the block deacidifying agent into a crusher for crushing to obtain deacidifying agent particles; (6) The deacidifying agent particles are added to a pulverizer for crushing, grinding, and sieving to obtain a finished deacidifying agent product. Example

[0015] (1) Add 30 parts of baking soda to 120 parts of water and fully dissolve to prepare a baking soda solution; (2) Add 40 parts of diatomaceous earth to the baking soda solution and stir slowly until it becomes a viscous liquid; (3) Add the liquid from step (2) into a mortar mixer, then add 5 parts of dispersant, 80 parts of calcium carbonate, and 15 parts of buffer, and stir for 30 minutes to obtain a premix; (4) The premix is ​​dried by low-temperature vacuum drying at a vacuum degree of 10 kPa, a drying temperature of 80°C, and a drying time of 90 min to remove the internal moisture and obtain a block deacidifying agent; (5) Adding the block deacidifying agent into a crusher for crushing to obtain deacidifying agent particles; (6) The deacidifying agent particles are added to a pulverizer for crushing, grinding, and sieving to obtain a finished deacidifying agent product. Example

[0016] (1) Add 30 parts of baking soda to 120 parts of water and fully dissolve to prepare a baking soda solution; (2) Add 35 parts of diatomaceous earth to the baking soda solution and stir slowly until it becomes a viscous liquid; (3) Add the liquid from step (2) into a mortar mixer, then add 4 parts of dispersant, 75 parts of calcium carbonate, and 12 parts of buffer, and stir for 25 minutes to obtain a premix; (4) The premix is ​​dried at low temperature and vacuum, with a vacuum degree of 8 kPa, a drying temperature of 70 ° C, and a drying time of 80 min to remove the internal moisture to obtain a block deacidification agent; (5) Adding the block deacidifying agent into a crusher for crushing to obtain deacidifying agent particles; (6) The deacidifying agent particles are added to a pulverizer for crushing, grinding, and sieving to obtain a finished deacidifying agent product.

[0017] In order to better illustrate the beneficial effects of the present invention, FIG1 is a process flow chart of the present invention, and the performance of the samples in the embodiments of the present invention was tested, mainly testing the specific surface area (BET), particle size (D50) and deacidification efficiency of the samples. The schematic diagram of the deacidification efficiency test device is shown in FIG2, and the test results are shown in Table 1.

[0018] Table 1 Performance test results of the samples in the embodiment:

Claims

1. A highly efficient furnace deacidification agent, It is characterized in that The composition includes (by weight): 20-40 parts of diatomaceous earth, 50-80 parts of calcium carbonate, 20-30 parts of baking soda, 10-15 parts of buffer, 3-5 parts of dispersant and 80-120 parts of water.

2. A method for preparing a highly efficient furnace deacidification agent, It is characterized in that The preparation comprises the following steps: (1) Add baking soda to water and fully dissolve it to prepare a baking soda solution; (2) adding diatomaceous earth to the baking soda solution prepared in step (1), and slowly stirring until a viscous liquid is obtained; (3) Add the viscous liquid obtained in step (2) into a blender, then add a dispersant, calcium carbonate, and a buffer, and stir for 15-30 minutes to obtain a premix; (4) removing the internal moisture of the premix prepared in step (3) by low-temperature vacuum drying to obtain a block deacidifying agent; (5) adding the block deacidifying agent obtained in step (4) into a crusher for crushing to obtain deacidifying agent particles; (6) Add the deacidifying agent particles obtained in step (5) into a pulverizer for crushing, grinding, and sieving to obtain a deacidifying agent finished product.

3. According to claim 1, a high-efficiency furnace deacidification agent, Features: The diatomaceous earth particle size is 30-100 μm.

4. A highly efficient furnace deacidification agent according to claim 1, Features: The calcium carbonate is light calcium carbonate with a particle size of 1-5 μm.

5. A high-efficiency furnace deacidification agent according to claim 1, Features: The buffer is one or more of sodium pyrophosphate, sodium hexametaphosphate and sodium tripolyphosphate.

6. A high-efficiency furnace deacidification agent according to claim 1, Features: The dispersant is a polymer dispersant, specifically one or more of polycarboxylate, maleic anhydride copolymer, and polyacrylic acid.

7. A high-efficiency furnace deacidification agent according to claim 2, Features: The drying process parameters of the preparation step (4) are as follows: vacuum degree 5-10 kPa, drying temperature 50-80° C., and drying time 60-90 min.

8. A method for preparing a high-efficiency furnace deacidification agent according to claim 2, Features: The sieve used in the preparation step (6) is 300-500 mesh.