Composite nanofiltration membrane as well as preparation method and application thereof
Through cross-linking reaction and multiple impregnation treatments, a composite nanofiltration membrane with narrow distribution and small pore size was formed. Combined with polytetrafluoroethylene aqueous dispersion, the problem of difficulty in intercepting small molecules of DMF in the existing nanofiltration membrane is solved, and efficient interception and industrialization are achieved Applicable effects.
Patent Information
- Application Number
- CN202411468712.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-21
- Publication Date
- 2024-11-29
AI Technical Summary
Existing nanofiltration membranes are difficult to effectively intercept small molecules DMF, and the preparation process is complicated and difficult to be used in industrial use.
The aqueous solution is formed by cross-linking of polyvinyl alcohol, maleic acid-containing compounds and styrenesulfonic acid-containing compounds. After multiple impregnation and heat treatment, a composite nanofiltration membrane with narrow distribution and small pore size is formed, combined with polytetrahydric acid-containing compounds. The vinyl fluoride aqueous dispersion forms a PTFE functional layer to build a composite nanofiltration membrane that is resistant to DMF dissolution.
It has achieved efficient interception of DMF in wastewater, and the preparation process is simple, suitable for industrial applications, has good polymer layer binding ability and environmental adaptability, and is suitable for acid/alkali and high-temperature conditions.
Smart Images

Figure CN119034506A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanofiltration membranes, and in particular to a composite nanofiltration membrane and a preparation method and application thereof. Background Art
[0002] Dimethylformamide (DMF, molecular weight 73) is a non-ionic short-chain tertiary amine organic compound with stable properties and is completely miscible in most organic solvents and water. DMF is widely used in petrochemical, printing and dyeing, and pharmaceutical industries as a raw material, extractant, gas absorbent, or cosolvent, and is therefore widely present in wastewater from related industries. The solubilization effect of DMF significantly inhibits the aggregation, volatilization, and precipitation of hydrophobic pollutants, resulting in a decrease in the flotation and coagulation removal efficiency of hydrophobic pollutants. Common coagulation, adsorption, oxidation, and other processes have the disadvantages of being time-consuming or having increased toxicity of intermediate products when treating DMF in wastewater.
[0003] Nanofiltration technology is a low-energy separation process that uses a specific pore size to size-screen organic matter of different molecular weights in aqueous solutions, and has shown great potential in removing small molecule pollutants from wastewater. However, the currently widely used commercial polyamide nanofiltration membranes, such as DuPont FilmTecTM NF270, are difficult to effectively intercept small molecules DMF due to their large pore size, and there is a problem that the functional layer on the surface of the nanofiltration membrane is easily dissolved by DMF.
[0004] Polytetrafluoroethylene (PTFE) is an organic polymer with excellent chemical stability and thermal stability, which is almost insoluble in any solvent. Due to the superior comprehensive properties of PTFE, it has become an ideal composite material for nanofiltration membranes to remove DMF from wastewater. However, the strong hydrophobicity and stable chemical properties lead to extremely poor processability of PTFE, and the preparation of PTFE functional layers and the regulation of pore structure are difficult. Therefore, selecting suitable materials to regulate the physical structure of the functional layer of the nanofiltration membrane is the main research direction for the preparation of high-efficiency composite nanofiltration membranes. Therefore, it is of great significance to provide a composite nanofiltration membrane that can effectively intercept small molecules of DMF in wastewater and is easy to prepare. Summary of the invention
[0005] The purpose of the present invention is to provide a composite nanofiltration membrane and a preparation method and application thereof, so as to achieve efficient interception of DMF in wastewater, and the preparation method of the composite nanofiltration membrane is simple and suitable for industrial application.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a composite nanofiltration membrane, comprising the following steps:
[0008] 1) mixing polyvinyl alcohol, a compound containing a maleic acid structure, a compound containing a styrene sulfonic acid structure and water, and performing a cross-linking reaction to obtain an aqueous phase solution;
[0009] 2) After the porous support layer is immersed in the aqueous solution, a first curing treatment is performed to obtain a primary composite nanofiltration membrane;
[0010] 3) After the primary composite nanofiltration membrane is immersed in a polytetrafluoroethylene aqueous dispersion, a second curing treatment is performed to obtain an intermediate composite nanofiltration membrane;
[0011] 4) After the intermediate composite nanofiltration membrane is immersed in the aqueous solution again, a third curing treatment is performed to obtain a composite nanofiltration membrane.
[0012] Optionally, the concentration of the polyvinyl alcohol in water is 1-10 g / L, the concentration of the compound containing maleic acid structure in water is 1-5 g / L; the concentration of the compound containing styrene sulfonic acid structure in water is 1-5 g / L.
[0013] Optionally, the polyvinyl alcohol is at least one of polyvinyl alcohol 105, polyvinyl alcohol 124, polyvinyl alcohol 224, polyvinyl alcohol 235 and polyvinyl alcohol 262;
[0014] The compound containing maleic acid structure is at least one of maleic acid, polymaleic acid and potassium maleate;
[0015] The compound containing styrene sulfonic acid structure is at least one of p-styrene sulfonic acid, sodium p-styrene sulfonate and sodium poly p-styrene sulfonate.
[0016] Optionally, the cross-linking reaction is carried out at a temperature of 70 to 100° C. and for a time of 2 to 12 hours.
[0017] Optionally, the solid content of the polytetrafluoroethylene aqueous dispersion is 0.7-8%;
[0018] The porous support layer is one of a porous polyimide support layer, a porous polyethylene support layer, a porous polyvinyl chloride support layer, a porous polypropylene support layer, a porous polysulfone support layer, a porous polyethersulfone support layer, and a porous polyacrylonitrile support layer;
[0019] The pore size of the porous support layer is 0.4-40 nm.
[0020] Optionally, the porous supporting layer is immersed in the aqueous solution for 5 to 30 minutes; the temperature of the first curing treatment is 50 to 100° C., and the time is 5 to 30 minutes.
[0021] Optionally, the primary composite nanofiltration membrane is immersed in the polytetrafluoroethylene aqueous dispersion for 5 to 30 minutes; the temperature of the second curing treatment is 50 to 100° C., and the time is 1 to 8 hours.
[0022] Optionally, the intermediate composite nanofiltration membrane is immersed in the aqueous solution again for 5 to 30 minutes; the temperature of the third curing treatment is 50 to 100° C., and the time is 5 to 30 minutes.
[0023] The present invention also provides a composite nanofiltration membrane prepared by the above preparation method.
[0024] The present invention also provides the use of the composite nanofiltration membrane in removing N,N-dimethylformamide (DMF) from wastewater.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention selects a widely used commercial nanofiltration membrane as a porous support layer, adopts an aqueous phase solution formed by crosslinking polyvinyl alcohol, a compound containing a maleic acid structure and a styrene sulfonic acid structure, and then impregnates it, and then heat-treats and solidifies it to form a three-dimensional network functional layer, the pore size of the nanofiltration membrane is initially reduced, and then the porous support layer is impregnated with a polytetrafluoroethylene aqueous dispersion, and then heat-treated and solidified to form a PTFE functional layer, which can effectively inhibit the dissolution of the nanofiltration membrane by DMF, and then impregnates the aqueous phase solution formed by crosslinking polyvinyl alcohol, a compound containing a maleic acid structure and a styrene sulfonic acid structure, and then heat-treats and solidifies it to form a three-dimensional network functional layer, and further constructs a composite nanofiltration membrane with a smaller pore structure, fewer defects and resistance to DMF dissolution. The method has strong controllability, simple operation, and mild process, and can construct membrane surface functional layers of different thicknesses according to the required flux and retention rate. This method can be used to prepare a composite nanofiltration membrane with narrow distribution of small pores and good polymer layer binding ability. The composite nanofiltration membrane is suitable for harsh environments and can efficiently intercept DMF in wastewater under acidic / alkaline (pH 4-10) and high temperature (temperature 20-60°C) conditions. The composite nanofiltration membrane can be used for deep treatment of wastewater containing small molecular impurities in industries such as petrochemicals, printing and dyeing, and medicine, and has broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 These are morphology characterization diagrams of the composite nanofiltration membrane of Example 1 of the present invention; wherein, (a) is a SEM image of the cross-sectional morphology of the composite nanofiltration membrane, and (b) is a SEM image of the surface morphology of the composite nanofiltration membrane.
[0028] Figure 2These are infrared spectrum analysis graphs and XPS spectrum analysis graphs of the composite nanofiltration membrane of Example 1 of the present invention; wherein, (a) is an infrared spectrum analysis graph of the composite nanofiltration membrane; (b) is an XPS wide spectrum analysis graph of the composite nanofiltration membrane; and (c) is an XPS narrow spectrum analysis graph of the composite nanofiltration membrane.
[0029] Figure 3 This is a graph showing the water contact angle data of the composite nanofiltration membrane of Example 1 of the present invention.
[0030] Figure 4 The graphs are the retention rate and pore size distribution of the composite nanofiltration membrane of Example 1 of the present invention for treating polyethylene glycols with different molecular weights; wherein (a) is the retention rate of the composite nanofiltration membrane for treating polyethylene glycols with different molecular weights, and (b) is the pore size distribution of the composite nanofiltration membrane.
[0031] Figure 5 1 is a zeta potential diagram of the composite nanofiltration membrane of Example 1 of the present invention at different pH values.
[0032] Figure 6 This is a pure water flux diagram of the composite nanofiltration membrane of Example 1 of the present invention under different operating pressures.
[0033] Figure 7 The figure is a graph of the retention rate of DMF wastewater of the composite nanofiltration membrane of Example 1 of the present invention at different pH and temperature; wherein, (a) is the retention rate of DMF wastewater treated by the composite nanofiltration membrane at different temperatures, and (b) is the retention rate of DMF wastewater treated by the composite nanofiltration membrane at different pH.
[0034] Figure 8 The membrane permeability diagram and retention rate diagram of the composite nanofiltration membrane in Example 1 of the present invention for the cyclic treatment of DMF wastewater; wherein, (a) is the membrane permeability of the composite nanofiltration membrane for treating DMF wastewater, and (b) is the retention rate of the composite nanofiltration membrane for treating DMF wastewater.
[0035] Fig. 9 This is a mass residual trend diagram of the composite nanofiltration membrane of Example 1 of the present invention in pure DMF. DETAILED DESCRIPTION
[0036] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0037] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0039] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0040] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0041] The raw materials used in the present invention can be obtained from the market or prepared by the existing technology.
[0042] The "room temperature" mentioned in the present invention is 25±2°C unless otherwise specified.
[0043] The present invention provides a method for preparing a composite nanofiltration membrane, comprising the following steps:
[0044] 1) mixing polyvinyl alcohol, a compound containing a maleic acid structure, a compound containing a styrene sulfonic acid structure and water, and performing a cross-linking reaction to obtain an aqueous phase solution;
[0045] 2) After the porous support layer is immersed in the aqueous solution, a first curing treatment is performed to obtain a primary composite nanofiltration membrane;
[0046] 3) After the primary composite nanofiltration membrane is immersed in a polytetrafluoroethylene aqueous dispersion, a second curing treatment is performed to obtain an intermediate composite nanofiltration membrane;
[0047] 4) After the intermediate composite nanofiltration membrane is immersed in the aqueous solution again, a third curing treatment is performed to obtain a composite nanofiltration membrane.
[0048] The invention firstly mixes polyvinyl alcohol, a compound containing a maleic acid structure, a compound containing a styrene sulfonic acid structure and water, and then performs a cross-linking reaction to obtain an aqueous phase solution.
[0049] In the present invention, there is no particular limitation on the mixing method, as long as the raw materials can be mixed uniformly. In the embodiment of the present invention, polyvinyl alcohol, the compound containing maleic acid structure, and the compound containing styrene sulfonic acid structure are directly dissolved in water.
[0050] In some embodiments of the present invention, the concentration of the polyvinyl alcohol in water is 1 to 10 g / L, preferably 2 to 8 g / L, more preferably 3 to 6 g / L, and even more preferably 4 to 5 g / L;
[0051] The concentration of the compound containing maleic acid structure in water is 1 to 5 g / L, preferably 2 to 4 g / L, and more preferably 3 to 3.5 g / L;
[0052] The concentration of the compound containing a styrene sulfonic acid structure in water is 1 to 5 g / L, preferably 2 to 4 g / L, and more preferably 3 to 3.5 g / L.
[0053] In some embodiments of the present invention, the polyvinyl alcohol is at least one of polyvinyl alcohol 105, polyvinyl alcohol 124, polyvinyl alcohol 224, polyvinyl alcohol 235 and polyvinyl alcohol 262;
[0054] The compound containing maleic acid structure is at least one of maleic acid, polymaleic acid and potassium maleate, preferably maleic acid;
[0055] The compound containing a styrene sulfonic acid structure is at least one of p-styrene sulfonic acid, sodium p-styrene sulfonate and sodium poly-p-styrene sulfonate, preferably sodium p-styrene sulfonate.
[0056] In some embodiments of the present invention, the temperature of the cross-linking reaction is 70-100° C., preferably 80-90° C., and the time is 2-12 h, preferably 3-10 h, and more preferably 4-6 h.
[0057] After obtaining the aqueous phase solution, the present invention immerses the porous support layer in the aqueous phase solution and then performs a first curing treatment to obtain a primary composite nanofiltration membrane.
[0058] In some embodiments of the present invention, after the porous supporting layer is immersed in the aqueous solution, the aqueous solution on its surface is removed, and then a first curing treatment is performed. The present invention does not limit the method of removing the aqueous solution, as long as the water can be removed. In the embodiments of the present invention, the surface aqueous solution is removed by natural air drying.
[0059] In some embodiments of the present invention, the porous support layer is immersed in the aqueous solution for 5 to 30 minutes, preferably 10 to 20 minutes; the temperature of the first curing treatment is 50 to 100°C, preferably 60 to 90°C, and further preferably 70 to 80°C, and the time is 5 to 30 minutes, preferably 10 to 20 minutes.
[0060] After obtaining the primary composite nanofiltration membrane, the present invention immerses the primary composite nanofiltration membrane in a polytetrafluoroethylene aqueous dispersion and then performs a second curing treatment to obtain an intermediate composite nanofiltration membrane;
[0061] In some embodiments of the present invention, after the primary composite nanofiltration membrane is immersed in the polytetrafluoroethylene aqueous dispersion, the polytetrafluoroethylene aqueous dispersion on its surface is removed, and then a second curing treatment is performed. The present invention does not specifically limit the method for removing the polytetrafluoroethylene aqueous dispersion, as long as the polytetrafluoroethylene aqueous dispersion can be removed. In the embodiments of the present invention, the surface aqueous phase solution is removed by natural air drying.
[0062] In the present invention, there is no limitation on the preparation method of the polytetrafluoroethylene aqueous dispersion, as long as the polytetrafluoroethylene aqueous dispersion with the required solid content can be obtained. In an embodiment of the present invention, the polytetrafluoroethylene aqueous dispersion is prepared by mixing a commercially available polytetrafluoroethylene dispersion (polytetrafluoroethylene dispersion in water) with water.
[0063] In some embodiments of the present invention, the solid content of the polytetrafluoroethylene dispersion is 40-80%, preferably 50-60%; the solid content of the polytetrafluoroethylene aqueous dispersion is 0.7-8%, preferably 2.86-7%, more preferably 3-6%, and even more preferably 4-5.45%.
[0064] In some embodiments of the present invention, the porous support layer is one of a porous polyimide support layer, a porous polyethylene support layer, a porous polyvinyl chloride support layer, a porous polypropylene support layer, a porous polysulfone support layer, a porous polyethersulfone support layer, and a porous polyacrylonitrile support layer, wherein the porous polyimide support layer includes products with models of DuPont NF90 and DuPont NF270. In an embodiment of the present invention, the porous support layer is a porous polyimide support layer, preferably DuPont NF270.
[0065] The pore size of the porous support layer of the present invention is 0.4 to 40 nm, preferably 0.45 to 20 nm, and more preferably 5 to 10 nm.
[0066] In some embodiments of the present invention, the primary composite nanofiltration membrane is immersed in the polytetrafluoroethylene aqueous dispersion for 5 to 30 minutes, preferably 10 to 20 minutes; the temperature of the second curing treatment is 50 to 100°C, preferably 60 to 90°C, and more preferably 70 to 80°C, and the time is 1 to 8 hours, preferably 2 to 6 hours, and more preferably 4 to 5 hours.
[0067] After obtaining the intermediate composite nanofiltration membrane, the present invention immerses the intermediate composite nanofiltration membrane in the aqueous solution again and then performs a third curing treatment to obtain a composite nanofiltration membrane.
[0068] In some embodiments of the present invention, after the intermediate composite nanofiltration membrane is immersed in the aqueous solution again, the aqueous solution on its surface is removed, and then a third curing treatment is performed. The present invention does not specifically limit the method for removing the aqueous solution, as long as the water can be removed. In the embodiments of the present invention, the surface aqueous solution is removed by natural air drying.
[0069] In some embodiments of the present invention, the intermediate composite nanofiltration membrane is immersed in the aqueous solution again for 5 to 30 minutes, preferably 10 to 20 minutes; the temperature of the third curing treatment is 50 to 100°C, preferably 60 to 90°C, and further preferably 70 to 80°C, and the time is 5 to 30 minutes, preferably 10 to 20 minutes.
[0070] In some embodiments of the present invention, after the third curing treatment is completed, the crude composite nanofiltration membrane obtained by the third curing treatment is washed to obtain a final composite nanofiltration membrane. The present invention has no particular limitation on the washing method, as long as the residual aqueous solution on the surface can be washed away. In an embodiment of the present invention, the crude composite nanofiltration membrane obtained after the third curing treatment is immersed in ultrapure water for washing to obtain the final composite nanofiltration membrane.
[0071] The present invention also provides a composite nanofiltration membrane prepared by the above preparation method.
[0072] The invention also provides application of the composite nanofiltration membrane in removing DMF from wastewater.
[0073] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0074] Example 1
[0075] 1) 0.2 g of polyvinyl alcohol 124, 0.5 g of maleic acid and 0.5 g of sodium p-styrene sulfonate were dissolved in 100 mL of water and stirred at 80° C. for 4 hours to perform a crosslinking reaction to obtain an aqueous phase solution.
[0076] 2) 5 mL of polytetrafluoroethylene dispersion with a solid content of 60% and 100 mL of water were mixed to obtain a polytetrafluoroethylene aqueous dispersion with a solid content of 2.86%.
[0077] 3) The DuPont NF270 nanofiltration membrane with a pore size of 0.45 nm was immersed in the aqueous solution for 10 minutes, the DuPont NF270 nanofiltration membrane after being immersed in the aqueous solution was taken out from the aqueous solution, the surface aqueous solution was removed by natural air drying, and then the membrane was cured at 80° C. for 10 minutes to obtain a primary composite nanofiltration membrane.
[0078] 4) After the temperature of the primary composite nanofiltration membrane drops to room temperature, the primary composite nanofiltration membrane is immersed in a polytetrafluoroethylene aqueous dispersion for 10 minutes, the polytetrafluoroethylene aqueous dispersion on the surface of the primary composite nanofiltration membrane after being immersed in the polytetrafluoroethylene aqueous dispersion is removed, and then the membrane is cured at 80° C. for 60 minutes to obtain an intermediate composite nanofiltration membrane.
[0079] 5) The obtained intermediate composite nanofiltration membrane was immersed in the aqueous solution again for 10 minutes, and the aqueous solution on the surface of the intermediate composite nanofiltration membrane after being immersed in the aqueous solution was removed, and then cured at 80° C. for 10 minutes. After the curing treatment, the crude composite nanofiltration membrane was immersed in ultrapure water for washing to obtain a composite nanofiltration membrane, and the pore size of the composite nanofiltration membrane was 0.22 nm.
[0080] The composite nanofiltration membrane was used to separate a 2 mmol / L DMF aqueous solution at 25°C, pH 7, and 0.8 MPa. The results showed that the DMF retention rate was 73.8% and the water permeation flux was 3.04 L·m -2 ·h -1 bar -1 .
[0081] Example 2
[0082] The only difference from Example 1 is that 10 mL of polytetrafluoroethylene emulsion (PTFE) with a solid content of 60% is dissolved in 100 mL of water to obtain a polytetrafluoroethylene aqueous dispersion with a solid content of 5.45%.
[0083] The composite nanofiltration membrane has a pore size of 0.19 nm. The separation results of the composite nanofiltration membrane for 2 mmol / L DMF at 25°C, pH 7, and 0.8 MPa are as follows: the DMF retention rate is 80.5%, and the water permeation flux is 0.86 L·m -2 ·h -1 bar-1 .
[0084] More functional layer accumulation will lead to smaller membrane pores. The composite nanofiltration membrane of Example 2 has a smaller pore size relative to the composite nanofiltration membrane of Example 1, which comes from the fact that more polytetrafluoroethylene is accumulated in layers in Example 2. Small membrane pores are beneficial for pollutant separation but not for water penetration. Therefore, the DMF retention rate of Example 2 is increased relative to Example 1, but the water permeation flux is reduced.
[0085] Example 3
[0086] The only difference from Example 1 is that 2 mL of polytetrafluoroethylene emulsion (PTFE) with a solid content of 60% is dissolved in 100 mL of water to obtain a polytetrafluoroethylene aqueous dispersion with a solid content of 1.18%.
[0087] The composite nanofiltration membrane has a pore size of 0.28 nm. The separation results of the composite nanofiltration membrane for 2 mmol / L DMF at 25°C, pH 7, and 0.8 MPa are as follows: the DMF retention rate is 35.8%, and the water permeation flux is 5.63 L·m -2 ·h -1 bar -1 .
[0088] Less functional layer accumulation will lead to larger membrane pores. The composite nanofiltration membrane of Example 3 has a larger pore size relative to the composite nanofiltration membrane of Example 1, which comes from less polytetrafluoroethylene accumulation in Example 3. Large membrane pores are not conducive to pollutant separation but are conducive to water permeation. Therefore, the DMF retention rate of Example 3 is reduced relative to Example 1, but the water permeation flux is increased.
[0089] Example 4
[0090] The only difference from Example 1 is that the added amount of sodium p-styrene sulfonate is 0.2 g.
[0091] The test showed that the pore size of the composite nanofiltration membrane was 0.24 nm. The separation results of the composite nanofiltration membrane for 2 mmol / LDMF at 25°C, pH 7, and 0.8 MPa were as follows: the DMF retention rate was 62.1%, and the water permeation flux was 4.36 L·m -2 ·h -1 bar -1 .
[0092] Sodium p-styrene sulfonate is one of the polymer monomers in the three-dimensional gel, and reducing the amount of sodium p-styrene sulfonate will lead to a larger pore size of the three-dimensional gel. Therefore, the DMF retention rate of Example 4 is reduced relative to that of Example 1, but the water permeation flux is increased.
[0093] Comparative Example 1
[0094] 1) 0.2 g of polyvinyl alcohol 124, 0.5 g of maleic acid and 0.5 g of sodium p-styrene sulfonate were dissolved in 100 mL of water and stirred at 80° C. for 4 hours to perform a crosslinking reaction to obtain an aqueous phase solution.
[0095] 2) The DuPont NF270 nanofiltration membrane with a pore size of 0.45 nm was immersed in the aqueous solution for 10 minutes. The DuPont NF270 nanofiltration membrane immersed in the aqueous solution was taken out from the aqueous solution, and the surface aqueous solution was removed by natural air drying, and then cured at 80° C. for 10 minutes. After the curing treatment was completed, the crude composite nanofiltration membrane obtained after the curing treatment was immersed in ultrapure water for washing to obtain a composite nanofiltration membrane modified with a single-layer three-dimensional network structure polymer layer.
[0096] The composite nanofiltration membrane has a pore size of 0.3 nm. The separation results of the composite nanofiltration membrane for 2 mmol / L DMF at 25°C, pH 7, and 0.8 MPa are as follows: the DMF retention rate is 18.6%, and the water permeation flux is 9.45 L·m -2 ·h -1 bar -1 .
[0097] Less functional layer accumulation will lead to larger membrane pores. The composite nanofiltration membrane of Comparative Example 1 has a larger pore size relative to the composite nanofiltration membrane of Example 1, which is derived from less polytetrafluoroethylene accumulation into layers and less three-dimensional network formation in Comparative Example 1. Large membrane pores are conducive to water penetration but not conducive to pollutant separation. Therefore, the DMF retention rate of Comparative Example 1 is reduced relative to Example 1, but the water permeation flux is increased.
[0098] Comparative Example 2
[0099] 1) Dissolve 5 mL of polytetrafluoroethylene dispersion with a solid content of 60% in 100 mL of water, and mix thoroughly to prepare a polytetrafluoroethylene aqueous dispersion with a solid content of 2.86%.
[0100] 2) A DuPont NF270 nanofiltration membrane with a pore size of 0.45 nm was immersed in a polytetrafluoroethylene aqueous dispersion for 10 minutes, the DuPont NF270 nanofiltration membrane immersed in the polytetrafluoroethylene aqueous dispersion was taken out from the polytetrafluoroethylene aqueous dispersion, the polytetrafluoroethylene aqueous dispersion on the surface was removed by natural air drying, and the membrane was cured at 80° C. for 60 minutes. After the curing treatment was completed, the crude composite nanofiltration membrane obtained after the curing treatment was immersed in ultrapure water for cleaning to obtain a composite nanofiltration membrane modified with a single-layer PTFE functional layer.
[0101] The composite nanofiltration membrane has a pore size of 0.29 nm. The separation results of the composite nanofiltration membrane for 2 mmol / LDMF at 25°C, pH 7, and 0.8 MPa are as follows: the DMF retention rate is 28.5%, and the water permeation flux is 3.8 L·m -2 ·h -1 bar -1 .
[0102] When the nanofiltration membrane is not immersed in the aqueous solution, there is no three-dimensional network functional layer on the surface of the nanofiltration membrane, and the composite nanofiltration membrane has a larger pore size. The large membrane pores are not conducive to the separation of pollutants but are conducive to water permeation. Therefore, the DMF retention rate of Comparative Example 2 is reduced relative to that of Example 1, but the water permeation flux is increased.
[0103] Comparative Example 3
[0104] 1) 0.2 g of polyvinyl alcohol, 0.5 g of maleic acid and 0.5 g of sodium p-styrene sulfonate were dissolved in 100 mL of water, and the mixture was stirred at 80° C. for 4 hours and then cross-linked to obtain an aqueous solution.
[0105] 2) Dissolve 5 mL of polytetrafluoroethylene dispersion with a solid content of 60% in 100 mL of water, mix thoroughly to prepare a polytetrafluoroethylene aqueous dispersion with a solid content of 2.86%.
[0106] 3) The DuPont NF270 nanofiltration membrane with a pore size of 0.45 nm was immersed in the aqueous solution for 10 minutes, the DuPont NF270 nanofiltration membrane after being immersed in the aqueous solution was taken out from the aqueous solution, the surface aqueous solution was removed by natural air drying, and then the membrane was cured at 80° C. for 10 minutes to obtain a primary composite nanofiltration membrane.
[0107] 4) After the temperature of the primary composite nanofiltration membrane drops to room temperature, the primary composite nanofiltration membrane is immersed in a polytetrafluoroethylene aqueous dispersion for 10 minutes, the polytetrafluoroethylene aqueous dispersion on the surface of the primary composite nanofiltration membrane after being immersed in the polytetrafluoroethylene aqueous dispersion is removed, and then the membrane is cured at 80° C. for 60 minutes. After the curing treatment is completed, the crude composite nanofiltration membrane obtained after the curing treatment is immersed in ultrapure water for cleaning to obtain a composite nanofiltration membrane that is not encapsulated with a three-dimensional network structure polymerization layer.
[0108] The test showed that the pore size of the composite nanofiltration membrane was 0.23 nm. The separation results of the composite nanofiltration membrane for 2 mmol / LDMF at 25°C, pH 7, and 0.8 MPa were as follows: the DMF retention rate was 53.2%, and the water permeation flux was 3.47 Lm -2 ·h -1 bar -1 .
[0109] Compared with Example 1, Comparative Example 3 lacks a three-dimensional network functional layer, so that the pore size of the prepared composite nanofiltration membrane is slightly larger than that of Example 1, so the retention rate of DMF is reduced and the water permeation flux is increased.
[0110] The present invention tests the structural properties and morphological characteristics of the composite nanofiltration membrane of Example 1, and the results are as follows: Figure 1-3 As shown by Figure 1 From (a) in FIG. 1 , it can be seen that the composite nanofiltration membrane presents a dense cross-sectional surface structure, that is, the multifunctional layer is tightly combined with the DuPont NF270 nanofiltration membrane; Figure 1 As can be seen from (b) in the figure, the composite nanofiltration membrane presents a uniform surface structure, that is, the multifunctional layer is evenly distributed without defects.
[0111] Depend on Figure 2 From (a) in the figure, it can be seen that the composite nanofiltration membrane surface has abundant CF and -SO3H functional groups; Figure 2 From (b) in the figure, we can see that the surface of the composite nanofiltration membrane contains C, N, O, and F elements. Figure 2 From (c) in the figure, it can be seen that the composite nanofiltration membrane surface has functional groups such as CC, C=O, CN and C-F2, which indicates that polytetrafluoroethylene and three-dimensional condensation are successfully loaded on the surface of DuPont NF270 nanofiltration membrane.
[0112] The present invention tested the water contact angle of the composite nanofiltration membrane prepared in Example 1. The test results are as follows: Figure 3 As shown in the figure, its water contact angle reaches 76° and its sliding contact angle reaches 88°. Although it is higher than the water contact angle and sliding contact angle of DuPont NF270 nanofiltration membrane, it is still less than 90°. It has wettability and sliding wettability, is easily wetted by water, and is conducive to intercepting impurities in water.
[0113] The present invention uses the composite nanofiltration membrane prepared in Example 1 to filter polyethylene glycols of different molecular weights to test the retention rate of different polyethylene glycols. In addition, the pore size distribution of the composite nanofiltration membrane prepared in Example 1 is tested. The test results are as follows: Figure 4 As shown by Figure 4 From (a), it can be seen that the composite nanofiltration membrane has a retention rate of more than 90% for 250Da polyethylene glycol; Figure 4 From (b), we can see that the pore size of the composite nanofiltration membrane is 0.22 nm.
[0114] The present invention tests the zeta potential of the composite nanofiltration membrane prepared in Example 1 at different pH values. The test results are as follows: Figure 5 As shown by Figure 5 It can be seen that the zeta potential of the composite nanofiltration membrane is negative under pH 3-11 conditions, and it has strong environmental adaptability.
[0115] The present invention tests the pure water flux of the composite nanofiltration membrane prepared in Example 1 under different operating pressures. The test results are as follows: Figure 6 As shown, it can be seen that the pure water flux of the composite nanofiltration membrane increases proportionally with the operating pressure and has stable water permeability.
[0116] The present invention tests the DMF retention rate of the composite nanofiltration membrane prepared in Example 1 at different pH and temperature. The test results are as follows: Figure 7 As shown by Figure 7 In (a), it can be seen that the retention rate of the composite nanofiltration membrane for DMF is 63.8-74.5% in the temperature range of 20-60°C; Figure 7 From (b), it can be seen that the retention rate of the composite nanofiltration membrane for DMF is 70-74.1% in the pH range of 4-10.
[0117] The present invention allows 1L of DMF aqueous solution with a concentration of 2mmol / L in the water inlet pool to pass through an area of 25cm 2 The composite nanofiltration membrane flows into the effluent pool, and the membrane permeability and retention rate are recorded. Then 0.25L of ultrapure water solution is sent back to the inlet pool through backwashing to clean the composite nanofiltration membrane. The above steps are repeated 5 times, and the membrane permeability and retention rate of the water solution passing through the composite nanofiltration membrane are recorded each time. The results are as follows Figure 8 As shown by Figure 8 From (a), we can see that the permeability of the composite nanofiltration membrane increases by 6.9% after 5 cycles; Figure 8 As shown in (b), the retention rate of DMF by the composite nanofiltration membrane decreased by 2.3% after 5 cycles, which indicates that the composite nanofiltration membrane has excellent cycle stability.
[0118] The present invention tests the quality residual trend of the composite nanofiltration membrane prepared in Example 1 in pure DMF. DuPont NF270 and the composite nanofiltration membrane are immersed in pure DMF for 7 days respectively. The results are as follows: Fig. 9 As shown, the numerical variation trend of the black squares in the figure shows that the mass residue of DuPont NF270 after immersion in pure DMF for 7 days is only 52%; the numerical variation trend of the hollow circles in the figure shows that the mass residue of the composite nanofiltration membrane after immersion in pure DMF for 7 days is 74%. This shows that the anti-solvent performance of the composite nanofiltration membrane is stronger than that of DuPont NF270. The same test was performed on the mass residue of the composite nanofiltration membrane obtained in other embodiments in pure DMF, and the results were similar, all showing high anti-solvent performance.
[0119] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a composite nanofiltration membrane, characterized in that: The following steps are involved: 1) mixing polyvinyl alcohol, a compound containing a maleic acid structure, a compound containing a styrene sulfonic acid structure and water, and performing a cross-linking reaction to obtain an aqueous phase solution; 2) After the porous support layer is immersed in the aqueous solution, a first curing treatment is performed to obtain a primary composite nanofiltration membrane; 3) After the primary composite nanofiltration membrane is immersed in a polytetrafluoroethylene aqueous dispersion, a second curing treatment is performed to obtain an intermediate composite nanofiltration membrane; 4) After the intermediate composite nanofiltration membrane is immersed in the aqueous solution again, a third curing treatment is performed to obtain a composite nanofiltration membrane.
2. The preparation method according to claim 1, characterized in that: The concentration of the polyvinyl alcohol in water is 1-10 g / L, the concentration of the compound containing maleic acid structure in water is 1-5 g / L; the concentration of the compound containing styrene sulfonic acid structure in water is 1-5 g / L.
3. The preparation method according to claim 2, characterized in that: The polyvinyl alcohol is at least one of polyvinyl alcohol 105, polyvinyl alcohol 124, polyvinyl alcohol 224, polyvinyl alcohol 235 and polyvinyl alcohol 262; The compound containing maleic acid structure is at least one of maleic acid, polymaleic acid and potassium maleate; The compound containing styrene sulfonic acid structure is at least one of p-styrene sulfonic acid, sodium p-styrene sulfonate and sodium poly p-styrene sulfonate.
4. The preparation method according to claim 1, characterized in that: The cross-linking reaction is carried out at a temperature of 70 to 100° C. and for a time of 2 to 12 hours.
5. The preparation method according to claim 1, characterized in that: The solid content of the polytetrafluoroethylene aqueous dispersion is 0.7-8%; The porous support layer is one of a porous polyimide support layer, a porous polyethylene support layer, a porous polyvinyl chloride support layer, a porous polypropylene support layer, a porous polysulfone support layer, a porous polyethersulfone support layer, and a porous polyacrylonitrile support layer; The pore size of the porous support layer is 0.4-40 nm.
6. The preparation method according to any one of claims 1 to 5, characterized in that The porous support layer is immersed in the aqueous solution for 5 to 30 minutes; the first curing treatment is performed at a temperature of 50 to 100° C. for 5 to 30 minutes.
7. The preparation method according to any one of claims 1 to 5, characterized in that The primary composite nanofiltration membrane is immersed in the polytetrafluoroethylene aqueous dispersion for 5 to 30 minutes; the temperature of the second curing treatment is 50 to 100° C. and the time is 1 to 8 hours.
8. The preparation method according to any one of claims 1 to 5, characterized in that The intermediate composite nanofiltration membrane is immersed in the aqueous solution again for 5 to 30 minutes; the temperature of the third curing treatment is 50 to 100° C. and the time is 5 to 30 minutes.
9. The composite nanofiltration membrane prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the composite nanofiltration membrane according to claim 9 in removing N,N-dimethylformamide from wastewater.