Cross-linked chitosan functionalized monolithic composite material as well as preparation method and application thereof
By forming crosslinked chitosan functionalized integral composite materials on the surface of nanosponges, the problem of low surface activity of nanosponges is solved, and the uniform loading of chitosan and efficient adsorption of heavy metal ions is achieved, which improves adsorption efficiency and recycling performance. , suitable for batch static and continuous dynamic adsorption applications.
Patent Information
- Application Number
- CN202411333706.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-29
AI Technical Summary
The existing nanosponges have low surface activity, resulting in uneven loading of chitosan, affecting adsorption efficiency and reusability, and the preparation process is complex and costly, making it difficult to achieve efficient removal of heavy metal ions by batch static adsorption and continuous dynamic adsorption.
By placing the nanosponge in a weakly alkaline buffer solution containing binder for ultrasonic self-polymerization, followed by adding glutaraldehyde and ammonia to the dilute acetic acid solution to form a crosslinked chitosan functionalized monolithic composite material, ensuring Chitosan is uniformly loaded and cross-linked to improve adsorption performance.
The chitosan has a reliable load and uniform load, and the material surface is rich in hydroxyl and amino functional groups, which significantly improves the batch static and continuous dynamic adsorption efficiency of heavy metal ions, maintains good recycling performance, is simple in process and low in cost, and is suitable for scale. Chemical production.
Smart Images

Figure CN119034688A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heavy metal ion removal in wastewater, and in particular to a cross-linked chitosan functionalized integral composite material and a preparation method and application thereof. Background Art
[0002] Among the methods for removing heavy metal ions from wastewater, the adsorption method has the advantages of simple operation, easy scalability, and no secondary pollution. In actual adsorption operations, the adsorption material is the key to the application of the adsorption method. The monolithic adsorption material combines the macroscopic overall structure with the microscopic active function, making its application have great potential. Under the premise of ensuring high adsorption efficiency, it is easy to achieve solid-liquid separation and recycling, and can also build a dynamic adsorption fixed column.
[0003] Since the cross-linked chitosan functionalized monolithic composite material has significant advantages in the field of removing heavy metals from wastewater, such as wide source of raw materials, low cost, high adsorption efficiency, batch static adsorption, and the ability to form a continuous flow adsorption device, it has a good application prospect in the field of wastewater treatment. Chitosan is a natural green polymer material that exhibits good biocompatibility and safety, making it widely used in many fields such as environment, medicine, food, and chemical industry. Its molecular structure contains a large number of hydroxyl and amino functional groups, strong chemical activity, and easy structure regulation, and has good adsorption performance. Commercialized nanosponge has low cost, controllable size, good elasticity, and a complete three-dimensional network structure at the microscopic level. The pores are well developed and easy to transfer mass in the liquid phase, making it a good choice as a monolithic substrate. Compared with the currently reported substrates such as activated carbon, silica gel, molecular sieves, nanomaterials, and metal oxides, nanosponge has a significant advantage in facilitating solid-liquid separation. Combining the macroscopic overall structure of nanosponge with the excellent adsorption performance of chitosan will broaden the application prospects.
[0004] However, the surface activity of nanosponge is low, and the preparation process of uniformly loading chitosan and firmly loading it on the nanosponge substrate is a major difficulty, which directly affects the adsorption efficiency, adsorption stability and reusability of the composite material. Chinese patent document CN116510706A discloses a preparation method and application of a porous nanosponge loaded MOF material, wherein the adsorption equilibrium time of the prepared porous nanosponge loaded MOF material is 150-500min, and the removal rate after 5 cycles decreases by 18.2%, and the adsorption rate and reusability need to be further improved.
[0005] Therefore, a chitosan-functionalized monolithic composite material with firm and uniform loading, simple synthesis process, low cost and easy scalability is developed, which has important practical application value for realizing batch static adsorption and continuous dynamic adsorption of heavy metal ions in wastewater. Summary of the invention
[0006] In view of this, the present invention provides a cross-linked chitosan functionalized monolithic composite material and a preparation method and application thereof. The synthesis process is simple and the cost is low, the chitosan loading is firm and the loading is uniform, and the prepared cross-linked chitosan functionalized monolithic composite material is used for removing heavy metals in wastewater in batch static adsorption and continuous flow adsorption modes.
[0007] The technical solution of the present invention is achieved as follows: A method for preparing a cross-linked chitosan functionalized monolithic composite material comprises the following steps:
[0008] S1, placing the nanosponge in a weakly alkaline buffer solution containing an adhesive, subjecting it to ultrasonication and constant temperature oscillation to cause a self-polymerization reaction, washing and drying, and obtaining a pre-modified adhesive / nanosponge monolithic composite material;
[0009] S2. placing the adhesive / nanosponge monolithic composite material in a dilute acetic acid solution containing chitosan, adding glutaraldehyde solution, heating and stirring, introducing ammonia gas to adjust the solution pH to 8-9, heating for reaction, washing and drying to obtain a cross-linked chitosan functional monolithic composite material.
[0010] Ammonia gas is introduced to adjust the pH of the solution to 8-9, so that the chitosan cross-linked by glutaraldehyde is physically deposited and modified on the surface of the adhesive / nanosponge monolithic composite material.
[0011] The adhesive is self-polymerized and coated on the surface of the nanosponge, making its surface rich in hydroxyl and amino functional groups, which is conducive to further modification. Chitosan is the product of chitin after deacetylation reaction, with a deacetylation degree greater than 95%, a high proportion of amino molecules and easy protonation of amino groups, which increases the solubility of chitosan in dilute acetic acid solution, and the volume concentration of dilute acetic acid solution is 2%. The above-mentioned cross-linked chitosan functionalized integral composite material uses nanosponge as the substrate, and is obtained by simple adhesive pre-modification and then chitosan cross-linked with glutaraldehyde through ammonia deposition.
[0012] Furthermore, in step S1, in order to ensure that the adhesive is uniformly dissolved in the buffer solution, the ultrasonic time is 3-10 min; in order to make the degree of self-polymerization reaction of the adhesive controllable, the reaction temperature of the constant temperature oscillation is 20-30°C, the reaction time is 2-4h, the pH value of the weak alkaline buffer solution is 8-9, and the concentration is 2-10mmol / L.
[0013] Furthermore, the mass ratio of the nanosponge to the adhesive is (0.20-1.00):(0.10-1.00), and the amount ratio of the buffer solution volume to the nanosponge is (50-300) mL:(0.20-1.00) g.
[0014] Furthermore, the adhesive is selected from any one of dopamine, catechol, catechol and gallic acid which can undergo self-polymerization reaction in weak alkaline buffer solution at room temperature.
[0015] Furthermore, the weakly alkaline buffer solution is any one of tris(hydroxymethyl)aminomethane hydrochloride, ammonia-ammonium chloride, and phosphate.
[0016] Furthermore, in step S2, the mass ratio of adhesive / nanosponge, chitosan and glutaraldehyde is (0.30-1.50):(0.20-1.00):(0.01-0.50).
[0017] Furthermore, in step S2, in order to ensure that chitosan and glutaraldehyde are fully cross-linked, the heating and stirring temperature is 50-80°C, and the reaction time is 60-180min; ammonia is introduced to adjust the pH of the solution to 8-9, and the heating reaction temperature is 50-80°C, and the reaction time is 60-180min.
[0018] A cross-linked chitosan functionalized integral composite material is prepared by the preparation method.
[0019] A cross-linked chitosan functionalized monolithic composite material is used for removing heavy metal ions from wastewater in batch static adsorption or continuous dynamic adsorption mode.
[0020] Beneficial effects of the present invention:
[0021] The invention provides a cross-linked chitosan functionalized integral composite material. The cross-linked chitosan functionalized integral composite material is based on a commercially available, inexpensive, easily available nano sponge (NS) with a three-dimensional network structure, developed pores and good elasticity. The nano sponge is pre-modified with a bonding adhesive (BA) to form a uniform coating layer on the surface of the nano sponge. Glutaraldehyde is added as a cross-linking agent, and after heating and stirring for a period of time, ammonia is introduced to physically deposit and modify the chitosan (CS) cross-linked by glutaraldehyde onto the surface of the coating layer, so as to obtain a cross-linked chitosan functionalized integral composite material (CS / BA@NS).
[0022] The cross-linked chitosan functionalized integral composite material prepared by the present invention retains the complete three-dimensional mesh through-hole structure of the nanosponge substrate, and realizes firm and uniform chitosan loading. The surface of the material is rich in hydroxyl and amino functional groups, and can achieve the purpose of efficiently removing heavy metal ions in batch static adsorption and continuous dynamic adsorption.
[0023] The cross-linked chitosan functionalized integral composite material prepared by the invention has good anti-elasticity, good chemical stability and excellent recycling performance; and the preparation process is simple, the cost is low, and it is suitable for large-scale production, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The physical picture and structural formula of CS / BA@NS prepared in Example 1;
[0025] Figure 2 Scanning electron microscopy images of CS / BA@NS and CS and BA@NS prepared in Example 1;
[0026] Figure 3 Fourier transform infrared spectra of CS / BA@NS and CS and BA@NS prepared in Example 1;
[0027] Figure 4 This is the radial and axial elastic properties diagram of CS / BA@NS prepared in Example 1.
[0028] Figure 5 Schematic diagram of the device for the adsorption experiment of CS / BA@NS prepared in Example 1;
[0029] Figure 6 This is a schematic diagram of the results of Application Example 1 of the present invention.
[0030] Figure 7 This is a schematic diagram of the results of Application Example 2 of the present invention.
[0031] Figure 8 This is a schematic diagram of the results of Application Example 3 of the present invention.
[0032] Fig. 9 This is a schematic diagram of the results of Application Example 4 of the present invention.
[0033] Fig.10 This is a schematic diagram of the results of Application Example 5 of the present invention. DETAILED DESCRIPTION
[0034] To make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described below with reference to the accompanying drawings.
[0035] Embodiment 1:
[0036] A method for preparing a cross-linked chitosan functionalized monolithic composite material comprises the following steps:
[0037] S1. Synthesis of adhesive / nanosponge monolithic composite material (BA@NS): Weigh 400 mg of NS and place it in 160 mL of phosphate buffer solution, the concentration of the phosphate buffer solution is 10 mmol / L, and the pH value is 8.5. Add 200 mg of dopamine, ultrasonicate for 5 min, and oscillate at 25°C for 3 h. For easy drying, wash with deionized water, then wash with anhydrous ethanol (density 0.79 g / mL), and dry at 70°C to obtain BA@NS;
[0038] S2. Synthesis of cross-linked chitosan functionalized monolithic composite material (CS / BA@NS): Weigh 200 mg chitosan and dissolve it in 50 mL dilute acetic acid solution (volume concentration is 2%) to obtain a dilute acetic acid solution containing chitosan; put 420 mg BA@NS prepared in step S1 into the dilute acetic acid solution containing chitosan, and add 0.01 g glutaraldehyde, heat and stir at 60°C for 60 min, pass ammonia to adjust the solution pH to 8, control the reaction temperature to 70°C, and the reaction time is 60 min. Then wash with deionized water and ethanol, dry at 70°C to obtain CS / BA@NS. The physical picture and structural formula of CS / BA@NS are as follows: Figure 1 shown.
[0039] The morphologies of NS, BA@NS and CS / BA@NS were characterized by SEM. Figure 2 As shown in the figure, NS is a 3D porous skeleton with a very smooth surface. After NS is treated with a weak alkaline solution containing BA, the skeleton of NS becomes rough and the surface is uniformly pre-modified. After BA@NS is modified by CS physical deposition cross-linked with GA, a thicker and rougher coating is loaded on the surface.
[0040] ATR FT-IR was used to characterize the functional groups of NS, BA@NS and CS / BA@NS. Figure 3 As shown. NS at 3320, 2943, 1543, 1149 and 810 cm -1 There are strong absorption peaks at 1457 and 1323 cm, which are NH bond stretching vibration, CH bond stretching vibration, C=N bond stretching vibration, CO bond stretching vibration and skeleton triazine ring bending vibration. -1 The absorption peak of BA@NS belongs to the bending vibration of CH bond. Due to the same skeleton structure, the main absorption peak of BA@NS is very similar to that of NS. However, after NS is pre-modified with BA, the absorption peak at 3320cm -1 The absorption peak of -1 1457cm -1 The absorption peak shifted to 1450cm -1 After the cross-linked CS was deposited on the surface of BA@NS, 3305cm -1 The absorption peak at 2916cm -1 The CH bond stretching vibration at 2850 and 1030 cm -1 Two new peaks appeared at , which corresponded to the symmetric stretching vibration of the CH bond and the stretching vibration of the CO bond in the primary alcohol. The above characterization results showed that CS / BA@NS was successfully prepared.
[0041] The compression-recovery experiment was used to verify the elastic properties of CS / BA@NS. The radial and axial directions were tested. The results are as follows: Figure 4 As shown in the figure. After 6 cycles of compression-recovery experiments, the shape of CS / BA@NS quickly recovered to its original state each time without collapse, indicating that it has good structural flexibility and stability. This advantage will enable CS / BA@NS to be used multiple times in batch static adsorption and continuous flow fixed column adsorption to effectively remove pollutants from wastewater.
[0042] Schematic diagram of batch static adsorption and continuous dynamic adsorption experimental device Figure 5 shown.
[0043] The cross-linked chitosan functionalized monolithic composite material CS / BA@NS prepared in Example 1 of the present invention is analyzed in conjunction with application examples.
[0044] Application Example 1:
[0045] Effect of cross-linked chitosan functionalized monolithic composite CS / BA@NS on heavy metal ions Pb 2+ Batch static adsorption:
[0046] Take 8 20mL ampoules, add 10mg of CS / BA@NS prepared in Example 1, and then add 20mL of Pb with concentrations of 25, 50, 75, 100, 125, 150, 175, and 200mg / L respectively. 2+ The pH of the solution was 5. After a contact time of 3 h at 25 °C, the CS / BA@NS was taken out and the remaining Pb in the filtrate was determined by atomic absorption spectrometry. 2+ According to the same ratio, the remaining Pb in the filtrate was measured at adsorption temperatures of 35°C and 45°C. 2+ concentration and calculated the adsorption amount.
[0047] The results are as follows Figure 6 As shown, Figure 6 (a) CS / BA@NS at 25℃, 35℃ and 45℃ for different Pb 2+ The adsorption amount of concentration; Figure 6 (b) is the linear fitting diagram of the Langmuir model, and (c) is the linear fitting diagram of the Freundlich model. Figure 6 It shows that CS / BA@NS has a significant effect on Pb 2+ With the increase of temperature, CS / BA@NS has a high adsorption capacity for Pb 2+ The adsorption amount of CS / BA@NS increased gradually, and the Langmuir and Freundlich linear fitting of thermodynamic adsorption models were consistent with the Langmuir model, indicating that CS / BA@NS has a good adsorption capacity for Pb 2+It is a monolayer adsorption.
[0048] Application Example 2:
[0049] Effect of cross-linked chitosan functionalized monolithic composite CS / BA@NS on heavy metal ions Pb 2+ Kinetic adsorption:
[0050] Take 8 20mL sample bottles, add 10mg CS / BA@NS prepared in Example 1, and then add 20mL 25mg / L Pb 2+ The solution was taken out at 25 °C after the contact time was 0, 5, 10, 20, 40, 60, 90, 120, and 180 min, and the remaining Pb in the filtrate was determined by atomic absorption spectrometry. 2+ According to the same ratio, the initial Pb 2+ The Pb content in the filtrate after contact with CS / BA@NS at different time concentrations of 75 mg / L and 200 mg / L 2+ concentration and calculated the adsorption amount.
[0051] The results are as follows Figure 7 As shown, Figure 7 (a) is the time-dependent adsorption curve of CS / BA@NS at 25 °C, (b) is the linear fitting diagram of the quasi-first-order model, and (c) is the linear fitting diagram of the quasi-second-order model. Figure 7 It shows that CS / BA@NS can 2+ Rapid adsorption. 2+ When the concentration is 25 mg / L, the equilibrium adsorption time is 60 min; when Pb 2+ When the concentration is 75 mg / L, the equilibrium adsorption time is 90 min; when Pb 2+ When the concentration was 200 mg / L, the equilibrium adsorption time was 120 min. The linear fitting of pseudo-first-order and pseudo-second-order adsorption kinetic models was consistent with the pseudo-second-order model, indicating that CS / BA@NS was effective for the adsorption of Pb 2+ It is chemical adsorption.
[0052] Application Example 3: Effect of ionic strength on the adsorption of heavy metal ions Pb by cross-linked chitosan functionalized monolithic composite CS / BA@NS 2+ Impact:
[0053] At 100 mg / L Pb 2+ 0, 20, 50, 100 mg / L Na was added to the solution + , K + , Ca 2+ or Mg 2+ The interfering ions and pH value were 5. The effects of CS / BA@NS on Pb2+ The effect of adsorption capacity. + or K + Under the action of CS / BA@NS, Pb 2+ There was no significant change in the adsorption capacity of Ca 2+ or Mg 2+ Will slightly affect CS / BA@NS to Pb 2+ The adsorption capacity of Ca 2+ or Mg 2+ The concentration of CS / BA@NS was 100 mg / L for Pb 2 + The adsorption capacity of ions decreased by 2.16% ( Figure 8 ), which is mainly due to Ca 2+ or Mg 2+ Competitive coordination with hydroxyl and amino groups in CS / BA@NS. 2+ The coordination interaction between them is strong, and external interfering ions will not significantly hinder the Pb 2+ adsorption.
[0054] Application example 4:
[0055] Continuous dynamic adsorption of heavy metal ions Pb by cross-linked chitosan functionalized monolithic composite CS / BA@NS 2+ :
[0056] Make a fixed column with a diameter of 2 cm and a height of 8 cm, and weigh 4 pieces of 2×2×2 cm 3 The CS / BA@NS is placed in the fixed column. Set Pb 2+ The concentrations of Pb were 5, 25, and 50 mg / L, respectively. 2+ The solution flows through the fixed column from bottom to top at a flow rate of 5 mL / min. The effluent is collected at fixed intervals and the Pb content in the filtrate is determined by atomic absorption spectrometry. 2+ Concentration. According to the influent concentration and effluent concentration (C t / C o ) versus time (t) to obtain the penetration curve, such as Fig. 9 (a) shown.
[0057] Using the same fixed column, set Pb 2+ The concentration of Pb is 5 mg / L. 2+ The solution flowed through the fixed column from bottom to top at 5, 8, and 10 mL / min, respectively. The effluent was collected at certain intervals and the Pb content in the filtrate was determined by atomic absorption spectrometry. 2+ concentration and draw a breakthrough curve, such as Fig. 9 (b) as shown.
[0058] The results are as follows Fig. 9 As shown, Fig. 9 The prepared CS / BA@NS was prepared at 25℃ with different Pb 2+ Concentration, breakthrough curves at different flow rates and model fitting diagrams. Fig. 9 It can be seen that all penetration curves present an S-shape. 2+ The lower the concentration, the slower the flow rate, the flatter the penetration curve, and the longer the penetration time and saturation time. 2+ Under load, the adsorption performance of the self-made fixed column is good and can remain constant until adsorption equilibrium. And by fitting the Thomas model and the Admas-Bohart model and comparing the correlation coefficient R values of the two models, it is shown that the Thomas model better describes the adsorption process of the CS / BA@NS fixed column, while the Admas-Bohart model can only describe the initial stage of the fixed column.
[0059] Application Example 5:
[0060] Effect of cross-linked chitosan functionalized monolithic composite CS / BA@NS on heavy metal ions Pb 2+ Cyclic performance:
[0061] Weigh 200 mg of CS / BA@NS prepared in Example 1 and add it to 400 mL of 25 mg / L Pb 2+ The solution (pH 5) was adsorbed at 25°C for 60 min, and the material was taken out. The remaining Pb in the filtrate was determined by atomic absorption spectrometry. 2+ The filtered material was washed with 0.1 mol / L Na2EDTA solution, then washed with deionized water and ethanol, and dried for the next recycling. Fig.10 As shown, Fig.10 It shows that in the first cycle, CS / BA@NS 2+ The removal rate reached 100%, and the removal rate after six cycles was greater than 92.5%, indicating that CS / BA@NS has excellent reusability.
[0062] Embodiment 2:
[0063] A method for preparing a cross-linked chitosan functionalized monolithic composite material comprises the following steps:
[0064] S1. Synthesis of BA / NS: Weigh 500 mg of NS and place it in 200 mL of tris(hydroxymethyl)aminomethane hydrochloride buffer solution with a concentration of 5 mmol / L and a pH value of 9.0. Add 200 mg of catechol, sonicate for 3 min, shake at 30°C for 2 h, wash with deionized water and ethanol, and dry at 70°C to obtain BA / NS;
[0065] S2, synthesis of CS / BA@NS: weigh 500 mg chitosan and dissolve it in 300 mL dilute acetic acid solution (volume concentration is 2%) to obtain a dilute acetic acid solution containing chitosan; put 520 mg BA@NS prepared in step S1 into the dilute acetic acid solution containing chitosan, and add 0.03 g glutaraldehyde, under continuous stirring, control the reaction temperature to 60°C, the reaction time to 80 min, introduce ammonia until the solution pH is 9.0, control the reaction temperature to 60°C, and the reaction time to 50 min. Then wash with deionized water and ethanol, and dry at 70°C to obtain CS / BA@NS.
[0066] Embodiment 3:
[0067] A method for preparing a cross-linked chitosan functionalized monolithic composite material comprises the following steps:
[0068] S1. Synthesis of BA / NS: Weigh 1000 mg of NS and place it in 300 mL of phosphate buffer solution with a concentration of 8 mmol / L and a pH value of 8.5. Add 500 mg of gallic acid, sonicate for 4 min, shake at 25°C for 4 h, wash with deionized water and ethanol, and dry at 70°C to obtain BA / NS;
[0069] S2, synthesis of CS / BA@NS: weigh 1000 mg chitosan and dissolve it in 500 mL dilute acetic acid solution (volume concentration is 2%) to obtain a dilute acetic acid solution containing chitosan; put 1050 mg BA@NS prepared in step S1 into the dilute acetic acid solution containing chitosan, and add 0.1 g glutaraldehyde, under continuous stirring, control the reaction temperature to 70°C, the reaction time to 120 min, introduce ammonia until the solution pH is 9.0, control the reaction temperature to 70°C, and the reaction time to 60 min. Then wash with deionized water and ethanol, and dry at 70°C to obtain CS / BA@NS.
[0070] The cross-linked chitosan functionalized monolithic composite material CS / BA@NS prepared by the present invention can efficiently remove heavy metal ions Pb in batch static adsorption and continuous dynamic adsorption. 2+ , static adsorption study of Pb 2+ The saturated adsorption capacity is as high as 174 mg / g. In addition, in the continuous flow adsorption study, at the set flow rate and influent concentration, the fixed column has a long saturation time and can maintain a good adsorption effect.
[0071] In the absence of conflict, the above embodiments and features in the embodiments may be combined with each other.
[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a cross-linked chitosan functionalized monolithic composite material, characterized in that: The following steps are involved: S1, placing the nanosponge in a weakly alkaline buffer solution containing an adhesive, subjecting it to ultrasonication and constant temperature oscillation to cause a self-polymerization reaction, washing and drying, and obtaining a pre-modified adhesive / nanosponge monolithic composite material; S2. placing the adhesive / nanosponge monolithic composite material in a dilute acetic acid solution containing chitosan, adding glutaraldehyde solution, heating and stirring, introducing ammonia gas to adjust the solution pH to 8-9, heating for reaction, and then washing and drying to obtain a cross-linked chitosan functional monolithic composite material.
2. The preparation method according to claim 1, characterized in that: In step S1, the ultrasonic time is 3-10 min, the reaction temperature of the constant temperature oscillation is 20-30° C., the reaction time is 2-4 h, the pH value of the weak alkaline buffer solution is 8-9, and the concentration is 2-10 mmol / L.
3. The preparation method according to claim 1 or 2, characterized in that: In step S1, the mass ratio of the nanosponge to the adhesive is (0.20-1.00):(0.10-1.00), and the volume ratio of the buffer solution to the nanosponge is (50-300) mL:(0.20-1.00) g.
4. The preparation method according to claim 1 or 2, characterized in that: The binder is any one of dopamine, catechol, catechol, and gallic acid.
5. The preparation method according to claim 1 or 3, characterized in that: The weakly alkaline buffer solution is any one of tris(hydroxymethyl)aminomethane hydrochloride, ammonia-ammonium chloride, and phosphate.
6. The preparation method according to claim 1, characterized in that: In step S2, the mass ratio of adhesive / nanosponge, chitosan and glutaraldehyde is (0.30-1.50):(0.20-1.00):(0.01-0.50).
7. The preparation method according to claim 1 or 6, characterized in that: In step S2, the temperature of heating and stirring is 50-80°C, and the reaction time is 60-180min; ammonia gas is introduced to adjust the pH of the solution to 8-9, and the heating reaction temperature is 50-80°C, and the reaction time is 60-180min.
8. A cross-linked chitosan functionalized monolithic composite material prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the cross-linked chitosan functionalized monolithic composite material according to claim 8 in removing heavy metal ions from wastewater in batch static adsorption or continuous dynamic adsorption mode.