Preparation method and application of surface molecularly imprinted membrane capable of selectively separating berberine
The preparation of the surface molecular imprinting film of berberine through surface molecular imprinting technology solves the problems of high operating costs and low efficiency in the treatment of berberine pharmaceutical wastewater, and achieves efficient and environmentally friendly selective separation of berberine, which is suitable for industrial production.
Patent Information
- Application Number
- CN202411346257.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art has problems of high operating costs and low efficiency when treating berberine pharmaceutical wastewater, making it difficult to achieve large-scale industrial production and pose a threat to environmental microorganisms.
Using surface molecular imprinting technology, using chitosan/polyvinyl alcohol composite film as a solid matrix, the functional monomer pre-acts with the template molecules, and the crosslinking agent and initiator are added to carry out stirring reaction under nitrogen protection conditions to prepare the curing reaction of Coptis chinensis. The molecular imprinting film on the surface of the protein achieves selective separation of berberine.
The prepared surface molecular imprinted film of berberine has high selective adsorption capacity, and the saturated adsorption amount reaches 74.56 mg/g. It has good biocompatibility, biodegradability and non-toxicity. It is suitable for industrial production, and the preparation process is simple and priced. Low cost, high processing efficiency, no secondary pollution.
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials and pharmaceutical wastewater treatment, and in particular to a preparation method and application of a surface molecular imprinting membrane capable of selectively separating berberine. Background Art
[0002] Berberine, as a natural isoquinoline alkaloid with multiple pharmacological and biological properties, is a widely used broad-spectrum antibacterial drug. It can be used clinically to treat digestive tract diseases and can also be used to inhibit viruses, protozoa, chlamydia and intestinal parasites. However, berberine pharmaceutical wastewater is a typical antibiotic wastewater. When the mass concentration of berberine in the wastewater is too high, it will produce strong toxicity, harm the microorganisms in the environment, destroy the population and community structure of microorganisms in the environment, and then destroy the original balance of the microecology in the environment, and even threaten human life and health (Martinez JL, Environmental Pollution, 2009, 157: 2893). At present, chemical, physicochemical and biochemical methods are the main methods for pharmaceutical wastewater treatment, but there are still limitations of high operating costs and low efficiency, which cannot be applied to industrial large-scale production.
[0003] Chitosan is a natural polymer derived from chitin. It has a unique molecular structure and is characterized by alkaline amino polysaccharides. It has good film-forming, biodegradable, and gas barrier capabilities. It also has antibacterial and antioxidant effects. It is a material with application prospects and is widely used in the field of wastewater treatment (Shi HX, Dong CY, Yang YY, Han YR, Wang F, WangCX, Men JY, International Journal of Biological Macromolecules, 2020, 163:2334). However, a single chitosan film cannot meet the requirements of mechanical properties of membrane materials. Polyvinyl alcohol is biodegradable, its film has high transparency, excellent gas barrier properties and mechanical properties, and is an environmentally friendly material that is widely used in the research of membrane materials. Researchers usually prepare chitosan and polyvinyl alcohol into chitosan / polyvinyl alcohol composite films, and prove that the performance of chitosan / polyvinyl alcohol composite films is outstandingly superior to that of simple polyvinyl alcohol films and chitosan films (Pan Qingyan, Zhou Chuang, Yang Ziming, He Zuyu, Wang Chao, Liu Yunhao, Song Shuhui, Gu Hui, Yu Lijuan, Li Xuerui, Qu Yunhui, Li Puwang, Food Research and Development, 2021, 42, 100).
[0004] Surface molecular imprinting polymers have a wide range of applications and high stability, and materials can be designed specifically according to different purposes and needs. Due to their special imprinting sites and specific functional groups, they can achieve selective recognition and specific binding of target molecules. The present invention uses chitosan / polyvinyl alcohol composite membrane as a solid matrix and adopts surface molecular imprinting technology to design a surface molecular imprinting membrane that can selectively separate berberine, which has a simple preparation process, stable performance, and is environmentally friendly. Summary of the invention
[0005] The technical problem to be solved by the present invention is: how to provide a surface molecular imprinting membrane which is simple in preparation process, low in price, stable in performance and environmentally friendly and can selectively separate berberine.
[0006] The technical solution adopted by the present invention is: A method for preparing a surface molecular imprinting membrane capable of selectively separating berberine, comprising the following steps: Step 1: pre-reacting the functional monomer with the template molecule, dissolving the template molecule berberine Ber and the functional monomer sodium p-styrene sulfonate SSS in water to react with each other to obtain a prepolymer; Step 2, preparation of surface molecular imprinting membrane, after soaking the chitosan / polyvinyl alcohol composite membrane in water to swell overnight, adding the prepolymer prepared in step 1, then adding the crosslinking agent, passing nitrogen to exhaust the air, adding the initiator, and continuously stirring the reaction under nitrogen protection to obtain the surface molecular imprinting membrane; Step three, eluting the template molecules, taking out the surface molecular imprinting membrane prepared in step two, repeatedly washing the membrane with an eluent to completely elute the template molecules, and vacuum drying to constant weight to obtain the berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM, which is a surface molecular imprinting membrane for selectively separating berberine.
[0007] In step 1, 6 grams of template molecule berberine Ber and 3.68 to 14.71 grams of functional monomer sodium styrene sulfonate SSS are added to each liter of water, and the mixture is stirred and reacted at 80° C. for 9 to 12 hours to obtain a prepolymer.
[0008] In step 2, the chitosan / polyvinyl alcohol composite film is soaked in water for swelling by soaking each gram of chitosan / polyvinyl alcohol composite film in 100 ml of water for swelling. When the prepolymer prepared in step 1 is added, the mass ratio of the template molecule berberine Ber to the chitosan / polyvinyl alcohol composite film is 2:1, the added cross-linking agent is N,N'-methylenebisacrylamide MBA, the added initiator is ammonium persulfate Aps, the reaction temperature is 75-90°C, and the reaction time is 8-11h.
[0009] The added cross-linking agent N,N'-methylenebisacrylamide MBA is 0.916-3.667 times the mass of the chitosan / polyvinyl alcohol composite film, and the added initiator ammonium persulfate Aps is 0.016-0.491 times the mass.
[0010] In step 3, the eluent is 1.5 mol / L sodium hydroxide solution.
[0011] The invention discloses an application of a surface molecular imprinting membrane capable of selectively separating berberine, characterized in that the berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM is applied in the selective adsorption of berberine.
[0012] The beneficial effects of the present invention are as follows: (1) The present invention adopts surface molecular imprinting technology to prepare berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM. Ber-PSSS@CS / PVA-SMIM can selectively adsorb berberine, with a saturated adsorption amount of 74.56 mg / g and an imprinting factor of 2.02. The imprinting factors for berberine structural analogs baicalein and tetracycline are 1.13 and 1.29, respectively. (2) The preparation process of the present invention uses chitosan / polyvinyl alcohol composite membrane as a solid matrix, which is green and harmless, has good biocompatibility, biodegradability and non-toxicity, has a wide source, and is suitable for industrial production requirements. (3) The preparation process of the present invention is simple, low-cost, easy to control, and the synthesis process can be completed completely in an aqueous solution. The prepared berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM has specific recognition selectivity and high binding affinity for berberine, and has stable performance, high processing efficiency, no secondary pollution, and can be recycled. DETAILED DESCRIPTION
[0013] Example 1: In a four-necked bottle, 0.3 g of chitosan / polyvinyl alcohol composite membrane was soaked in 30 mL of water and swollen overnight. 0.6 g of template molecule berberine Ber and 0.736 g of functional monomer sodium p-styrene sulfonate SSS were dissolved in 100 mL of water at 80°C and interacted for 12 h to obtain a prepolymer, which was added to the above four-necked bottle. Then 0.825 g of cross-linker N,N'-methylenebisacrylamide MBA was added, and nitrogen was passed for 30 minutes to exhaust the air. 0.00736 g of initiator ammonium persulfate Aps was dissolved in 5 mL of distilled water and slowly added to the above four-necked bottle. The temperature was raised to 80°C under nitrogen protection and stirred for 9 h. After the reaction, the membrane was taken out and repeatedly soaked and cleaned with 1.5 mol / L sodium hydroxide solution to completely elute the template molecule, and then vacuum dried to constant weight to obtain berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM.
[0014] At the same time, a non-molecular imprinting membrane (SNIM) was prepared in the same manner as above except that the template molecule berberine Ber was not added.
[0015] Take 25 mL of berberine solution with a concentration of 1.8 mg / mL in a conical flask, add 0.05 g of imprinted membrane Ber-PSSS@CS / PVA-SMIM and 0.05 g of non-molecular imprinted membrane SNIM respectively, place it in a constant temperature oscillator, and oscillate at a constant temperature of 25°C for 2 h. The saturated adsorption capacity of the imprinted membrane Ber-PSSS@CS / PVA-SMIM can reach 74.56 mg / g, while the saturated adsorption capacity of the non-molecular imprinted membrane SNIM is 36.91 mg / g.
[0016] Example 2: In a four-necked bottle, 0.3 g of chitosan / polyvinyl alcohol composite membrane was soaked in 30 mL of water and swollen overnight. 0.6 g of template molecule berberine Ber and 0.368 g of functional monomer sodium p-styrene sulfonate SSS were dissolved in 100 mL of water at 80°C and interacted for 9 h to obtain a prepolymer, which was added to the above four-necked bottle. Then 0.275 g of cross-linker N,N'-methylenebisacrylamide MBA was added, and nitrogen was passed for 30 minutes to exhaust the air. 0.005 g of initiator ammonium persulfate Aps was dissolved in 5 mL of distilled water and slowly added to the above four-necked bottle. The temperature was raised to 75°C under nitrogen protection and stirred for 8 h. After the reaction was completed, the membrane was taken out and repeatedly soaked and cleaned with 1.5 mol / L sodium hydroxide solution to completely elute the template molecule, and then vacuum dried to constant weight to obtain berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM. At the same time, a non-molecular imprinting membrane (SNIM) was prepared in the same manner as above except that the template molecule berberine Ber was not added.
[0017] Take 25 mL of berberine solution with a concentration of 1.8 mg / mL in a conical flask, add 0.05 g of imprinted membrane Ber-PSSS@CS / PVA-SMIM and 0.05 g of non-molecular imprinted membrane SNIM respectively, place it in a constant temperature oscillator, and oscillate at a constant temperature of 25°C for 2 h. The saturated adsorption capacity of the imprinted membrane Ber-PSSS@CS / PVA-SMIM can reach 66.71 mg / g, while the saturated adsorption capacity of the non-molecular imprinted membrane SNIM is 33.82 mg / g.
[0018] Example 3: In a four-necked bottle, 0.3 g of chitosan / polyvinyl alcohol composite membrane was soaked in 30 mL of water and swollen overnight. 0.6 g of template molecule berberine Ber and 1.103 g of functional monomer sodium p-styrene sulfonate SSS were dissolved in 100 mL of water at 80 ° C for 10 h to obtain a prepolymer, which was added to the above four-necked bottle. Then 0.550 g of cross-linker N,N'-methylenebisacrylamide MBA was added, and nitrogen was passed for 30 minutes to exhaust the air. 0.0110 g of initiator ammonium persulfate Aps was dissolved in 5 mL of distilled water and slowly added to the above four-necked bottle. The temperature was raised to 85 ° C under nitrogen protection and stirred for 10 h. After the reaction, the membrane was taken out and repeatedly soaked and cleaned with 1.5 mol / L sodium hydroxide solution to completely elute the template molecule, and then vacuum dried to constant weight to obtain berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM. At the same time, a non-molecular imprinting membrane (SNIM) was prepared in the same manner as above except that the template molecule berberine Ber was not added.
[0019] Take 25 mL of 1.8 mg / mL berberine solution in a conical flask, add 0.05 g imprinted membrane Ber-PSSS@CS / PVA-SMIM and 0.05 g non-molecular imprinted membrane SNIM respectively, place it in a constant temperature oscillator, and oscillate at 25°C for 2 h. The saturated adsorption capacity of the imprinted membrane Ber-PSSS@CS / PVA-SMIM can reach 70.48 mg / g, while the saturated adsorption capacity of the non-molecular imprinted membrane SNIM is 35.17 mg / g.
[0020] Example 4: In a four-necked bottle, 0.3 g of chitosan / polyvinyl alcohol composite membrane was soaked in 30 mL of water and swollen overnight. 0.6 g of template molecule berberine Ber and 1.471 g of functional monomer sodium p-styrene sulfonate SSS were dissolved in 100 mL of water at 80°C and interacted for 11 h to obtain a prepolymer, which was added to the above four-necked bottle. Then 1.100 g of cross-linker N,N'-methylenebisacrylamide MBA was added, and nitrogen was passed for 30 minutes to exhaust the air. 0.0147 g of initiator ammonium persulfate Aps was dissolved in 5 mL of distilled water and slowly added to the above four-necked bottle. The temperature was raised to 90°C under nitrogen protection and stirred for 11 h. After the reaction, the membrane was taken out and repeatedly soaked and cleaned with 1.5 mol / L sodium hydroxide solution to completely elute the template molecule, and then vacuum dried to constant weight to obtain berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM. At the same time, a non-molecular imprinting membrane (SNIM) was prepared in the same manner as above except that the template molecule berberine Ber was not added.
[0021] Take 25 mL of 1.8 mg / mL berberine solution in a conical flask, add 0.05 g imprinted membrane Ber-PSSS@CS / PVA-SMIM and 0.05 g non-molecular imprinted membrane SNIM respectively, place it in a constant temperature oscillator, and oscillate at 25°C for 2 h. The saturated adsorption capacity of the imprinted membrane Ber-PSSS@CS / PVA-SMIM can reach 69.24 mg / g, while the saturated adsorption capacity of the non-molecular imprinted membrane SNIM is 34.57 mg / g.
[0022] It can be seen from the above examples that the saturated adsorption capacity of the imprinted membrane Ber-PSSS@CS / PVA-SMIM is greater than 66 mg / g, and the maximum can reach 74.56 mg / g, while the saturated adsorption capacity of the non-molecular imprinted membrane SNIM is greater than 33.8 mg / g, and the maximum can reach 36.91 mg / g.
Claims
1. A method for preparing a surface molecular imprinted membrane capable of selectively separating berberine, characterized in that: The following steps are included Step 1: pre-reacting the functional monomer with the template molecule, dissolving the template molecule berberine Ber and the functional monomer sodium p-styrene sulfonate SSS in water to react with each other to obtain a prepolymer; Step 2, preparation of surface molecular imprinting membrane, after soaking the chitosan / polyvinyl alcohol composite membrane in water to swell overnight, adding the prepolymer prepared in step 1, then adding the crosslinking agent, passing nitrogen to exhaust the air, adding the initiator, and continuously stirring the reaction under nitrogen protection to obtain the surface molecular imprinting membrane; Step three, eluting the template molecules, taking out the surface molecular imprinting membrane prepared in step two, repeatedly washing the membrane with an eluent to completely elute the template molecules, and vacuum drying to constant weight to obtain the berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM, which is a surface molecular imprinting membrane for selectively separating berberine.
2. The method for preparing a surface molecular imprinted membrane capable of selectively separating berberine according to claim 1, characterized in that: In step 1, 6 grams of template molecule berberine Ber and 3.68 to 14.71 grams of functional monomer sodium styrene sulfonate SSS are added to each liter of water, and the mixture is stirred and reacted at 80° C. for 9 to 12 hours to obtain a prepolymer.
3. The method for preparing a surface molecular imprinted membrane capable of selectively separating berberine according to claim 1, characterized in that: In step 2, the chitosan / polyvinyl alcohol composite film is soaked in water for swelling by soaking each gram of chitosan / polyvinyl alcohol composite film in 100 ml of water for swelling. When the prepolymer prepared in step 1 is added, the mass ratio of the template molecule berberine Ber to the chitosan / polyvinyl alcohol composite film is 2:1, the added cross-linking agent is N,N'-methylenebisacrylamide MBA, the added initiator is ammonium persulfate Aps, the reaction temperature is 75-90°C, and the stirring reaction time is 8-11h.
4. The method for preparing a surface molecular imprinted membrane capable of selectively separating berberine according to claim 3, characterized in that: The added cross-linking agent N,N'-methylenebisacrylamide MBA is 0.916-3.667 times the mass of the chitosan / polyvinyl alcohol composite film, and the added initiator ammonium persulfate Aps is 0.016-0.491 times the mass.
5. The method for preparing a surface molecular imprinted membrane capable of selectively separating berberine according to claim 1, characterized in that: In step 3, the eluent is 1.5 mol / L sodium hydroxide solution.
6. An application of a surface molecular imprinting membrane for selectively separating berberine prepared by the method of claim 1, characterized in that: Application of berberine surface molecular imprinting membrane Ber-PSSS@CS / PVA-SMIM in selective adsorption of berberine.
Citation Information
Patent Citations
Preparation method of matrine molecule surface blotting polymer material
CN103601910A
Preparation method of biomass-based molecularly imprinted composite membrane for selectively separating tetracycline
CN111004411A