Indium zirconium oxide loaded monatomic platinum catalyst and preparation method and application thereof
By using ammonium carbonate precipitation method in carbon dioxide hydrogenation catalyst and supporting single-atom platinum through the immersion method, the problem of insufficient catalyst activity and selectivity is solved, efficient carbon dioxide conversion and methanol selectivity is achieved, and good Stability and heat resistance.
Patent Information
- Application Number
- CN202411157109.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
The existing carbon dioxide hydrogenation catalysts have low activity, low selectivity of methanol and poor stability, making it difficult to achieve efficient catalytic reactions under mild conditions.
Indium zirconium oxide is prepared by precipitation method using ammonium carbonate as a precipitant, and single-atom platinum is supported on its surface by impregnation method to form an indium zirconium oxide-supported single-atom platinum catalyst to improve catalytic activity and selectivity.
It significantly improves the catalytic activity of the catalyst and the selectivity of methanol, extends the catalytic life, reduces by-products, achieves high conversion of carbon dioxide and high selectivity of methanol, and has heat resistance and stability.
Smart Images

Figure CN119034727A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalysts, and in particular relates to an indium zirconium oxide-supported single-atom platinum catalyst and a preparation method and application thereof. Background Art
[0002] Catalytic reduction of carbon dioxide can produce a variety of high-value basic chemicals and reduce the carbon dioxide content in the atmosphere. Using light, electricity, heat and other energy sources, hydrogen is produced using renewable energy hydrogen production technology, and the highly oxidized carbon in carbon dioxide is reduced to reusable carbon-containing resource products under the action of catalysts. Among the many CO2 catalytic conversion processes, the CO2 catalytic hydrogenation process has the largest demand.
[0003] Among the many high-value-added chemicals synthesized by CO2 hydrogenation, methanol can be used as a fuel in internal combustion engines and fuel cells. Methanol, as a C1 compound, is an intermediate product for the synthesis of other important chemicals. Cu-based catalysts are the most commonly used and widely studied catalysts for the synthesis of methanol by CO2 hydrogenation. However, under the influence of the byproduct H2O, the ZnO on the surface of the Cu / ZnO / Al2O3 catalyst is easily agglomerated and the copper particles are easily oxidized, which leads to serious deactivation. Precious metal-based catalysts are potential candidate catalysts for low-temperature CO2 hydrogenation to methanol. Low-temperature reactions are more thermodynamically favorable for the production of methanol. However, due to the weak CO2 binding, precious metal catalysts cannot change the product distribution when used alone in the catalytic reaction, and their methanol selectivity and conversion rate still need to be further improved.
[0004] Currently, CO2 hydrogenation catalysts still have problems such as low activity, low selectivity for methanol and poor stability. Therefore, it is urgent to develop CO2 hydrogenation catalysts with high activity, high selectivity and high stability under milder conditions. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an indium zirconium oxide supported single-atom platinum catalyst and its preparation method and application. The catalyst prepared by the preparation method of the present invention has high catalytic activity, carbon dioxide conversion rate and methanol selectivity, and has the characteristics of long catalytic life and less by-products.
[0006] The inventive concept of the present invention is as follows: the present invention first uses ammonium carbonate as a precipitant and adopts a precipitation method to prepare indium zirconium oxide. Compared with other precipitants, ammonium carbonate has a higher carbon dioxide conversion rate and methanol selectivity, which is beneficial to improve the space-time yield of methanol; then an impregnation method is adopted to load platinum with good catalytic activity on the surface of indium zirconium oxide in the form of a single atom, thereby greatly improving the catalytic activity of the catalyst and further improving the selectivity of methanol. Therefore, the indium zirconium oxide loaded single-atom platinum catalyst for synthesizing methanol by hydrogenation of carbon dioxide prepared by the present invention has a good ability to adsorb and activate CO2, and stabilizes the active intermediates, so that it mainly generates methanol instead of reverse water gas reaction; and the catalyst has a high ability to crack H2, which promotes the reaction of hydrogen after cracking with the intermediate to generate methanol, thereby improving the selectivity of methanol. At the same time, due to the stability of indium zirconium oxide itself, the catalyst of the present invention also has the characteristics of strong heat resistance, anti-sintering, good stability, etc.
[0007] In order to solve the above technical problems, the first aspect of the present invention provides a method for preparing a catalyst, comprising the following steps:
[0008] (1) dissolving an indium source, a zirconium source and a precipitant in water, adjusting the pH value, standing for aging, filtering, washing, drying and calcining to obtain indium zirconium oxide; the precipitant is ammonium carbonate;
[0009] (2) The indium zirconium oxide is immersed in an aqueous solution of a platinum source, mixed, and dried; and then the dried solid is ground and calcined to obtain the catalyst.
[0010] Preferably, the indium source comprises indium nitrate tetrahydrate.
[0011] Preferably, the zirconium source is selected from at least one of zirconium nitrate pentahydrate, zirconium oxynitrate pentahydrate, zirconium oxychloride and zirconium oxide.
[0012] Preferably, the molar ratio of the indium source to the zirconium source is (1-3):1.
[0013] Preferably, the molar ratio of the zirconium source to the precipitant is 1:(2-4).
[0014] Preferably, the indium source, the zirconium source and the precipitant are dissolved in water to form a solution, and the concentration of the zirconium source is 0.01-0.1 mol / L.
[0015] Preferably, in the aqueous solution of the platinum source, the solute is selected from at least one of platinum nitrate, chloroplatinic acid and ammonium chloroplatinate.
[0016] Preferably, the concentration of the aqueous solution of the platinum source is 0.0025-0.025 mol / L.
[0017] Preferably, the mass volume ratio of the indium zirconium oxide to the aqueous solution of the platinum source is (1-2) g:1 mL.
[0018] Preferably, in step (1), the pH value is 7-8.
[0019] Preferably, in step (1), the static aging time is 1-3 hours.
[0020] Preferably, in step (1), the washing is performed with deionized water for 2-4 times.
[0021] Preferably, in step (1), the drying is performed at 70-90° C. for 10-15 hours.
[0022] Preferably, in step (1), the calcination temperature condition is: calcination at 450-550° C. for 2-4 hours.
[0023] Preferably, in step (2), the drying is performed at 70-90° C. for 8-12 hours.
[0024] Preferably, in step (2), the calcination temperature condition is: calcination at 450-550° C. for 2-4 hours.
[0025] The second aspect of the present invention provides a catalyst prepared by the above-mentioned preparation method, wherein the catalyst comprises indium zirconium oxide and single-atom platinum, and the single-atom platinum is uniformly loaded on the surface of the indium zirconium oxide. In the catalyst of the present invention, the noble metal platinum is uniformly distributed on the surface of the indium zirconium oxide in the form of single atoms, which is conducive to promoting the activation and dissociation of carbon dioxide and hydrogen, and significantly improving the efficiency of the catalytic reaction.
[0026] Preferably, the loading amount of the single-atom platinum is 0.01-4wt%; more preferably, the loading amount of the single-atom platinum is 0.01-0.1wt%. The loading amount in the present invention refers to the mass proportion of the single-atom platinum in the catalyst.
[0027] A third aspect of the present invention provides a method for preparing methanol by hydrogenating carbon dioxide, comprising the following steps:
[0028] The catalyst is placed in a reactor, hydrogen and carbon dioxide are introduced, the temperature and pressure are increased, and the reaction is carried out to obtain the methanol.
[0029] Preferably, the temperature is raised to 235-315°C.
[0030] Preferably, the pressure is increased to 1-4 MPa.
[0031] Preferably, the flow rate of hydrogen and carbon dioxide is 6000-18000h -1 .
[0032] Preferably, the molar ratio of hydrogen to carbon dioxide is (1-5):1.
[0033] Preferably, before the introduction of hydrogen and carbon dioxide, the method further comprises activating the catalyst at 200-400° C. for 0.5-1 hour in argon at normal pressure, with the flow rate of the argon being 20-40 mL / min.
[0034] Compared with the prior art, the above technical solution of the present invention has at least the following technical effects or advantages:
[0035] (1) In the process of preparing the catalyst of the present invention, a specific ammonium carbonate is first used as a precipitant to prepare indium zirconium oxide by a precipitation method, so as to improve the catalyst's conversion rate to carbon dioxide and selectivity to methanol, thereby improving the space-time yield of methanol; then an impregnation method is used to load platinum in the form of a single atom on the surface of the indium zirconium oxide, thereby greatly promoting the activation and dissociation of carbon dioxide and hydrogen, and significantly improving the efficiency of the catalytic reaction.
[0036] (2) The catalyst prepared by the present invention has good ability to adsorb and activate CO2, and stabilize active intermediates, so that when it is used in the carbon dioxide hydrogenation reaction, it mainly produces methanol instead of a reverse water gas reaction; and the catalyst has a high ability to crack H2, promoting the reaction of the cracked hydrogen with the intermediate to produce methanol, thereby improving the selectivity of methanol, achieving a carbon dioxide conversion rate of 11.00-14.20%, a methanol selectivity of 93.20-97.50%, and a methanol space-time yield of 0.521754-0.704541 gMeOH / g·h. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 TEM image of the catalyst prepared in Example 1 of the present invention;
[0038] Figure 2 XRD diagrams of the catalyst and indium zirconium oxide prepared in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0039] The present invention is described in detail below in conjunction with the examples, so that the technical personnel of the relevant technical field can understand the present invention. It is necessary to point out here that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The non-essential improvements and adjustments made to the present invention by the skilled person in the relevant field according to the above invention content should still belong to the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods that are not mentioned in detail are all process steps or preparation methods known to those skilled in the art.
[0040] Example 1
[0041] A method for preparing an indium zirconium oxide-supported single-atom platinum catalyst comprises the following steps:
[0042] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.0375mol (NH4)2CO3 in 100mL H2O to form precipitant solution B; add these two solutions to a four-necked flask at a certain flow rate in a 70℃ water bath, and keep the pH of the solution at 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an 80℃ oven for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0043] H 12 N6O6 platinum powder was dissolved in distilled water to make 0.0025-0.025 mol / L H 12 N6O6 platinum aqueous solution. Take 198.5ul H 12 The N6O6 platinum aqueous solution was added to 50 mL of H2O, and then 1 g of powdered indium zirconium oxide was immersed in the prepared H2O. 12 N6O6 platinum aqueous solution, stirred at room temperature for 3 hours. The obtained supported platinum indium zirconium oxide was dried in an oven at 80°C for 8-12 hours, and the solid was ground into powder after drying, and then the powder was calcined in a muffle furnace at 500°C for 3 hours to obtain an indium zirconium oxide supported single atom platinum catalyst with a platinum loading of 0.01%.
[0044] Example 2
[0045] A method for preparing an indium zirconium oxide-supported single-atom platinum catalyst comprises the following steps:
[0046] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.0375mol (NH4)2CO3 in 100mL H2O to form precipitant solution B; add these two solutions to a four-necked flask at a certain flow rate in a 70℃ water bath, and keep the pH of the solution at 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an 80℃ oven for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0047] H 12 N6O6 platinum powder was dissolved in distilled water to make 0.0025-0.025 mol / L H 12N6O6 platinum aqueous solution. Take 595.5ul H 12 The N6O6 platinum aqueous solution was added to 50 mL of H2O, and then 1 g of powdered indium zirconium oxide was immersed in the prepared H2O. 12 N6O6 platinum aqueous solution, stirred at room temperature for 3 hours. The obtained platinum-loaded indium zirconium oxide was dried in an oven at 80°C for 8-12 hours, and the solid was ground into powder after drying, and then the powder was calcined in a muffle furnace at 500°C for 3 hours to obtain an indium zirconium oxide-loaded single-atom platinum catalyst with a platinum loading of 0.03%.
[0048] Example 3
[0049] A method for preparing an indium zirconium oxide-supported single-atom platinum catalyst comprises the following steps:
[0050] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.0375mol (NH4)2CO3 in 100mL H2O to form precipitant solution B; add these two solutions to a four-necked flask at a certain flow rate in a 70℃ water bath, and keep the pH of the solution at 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an 80℃ oven for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0051] H 12 N6O6 platinum powder was dissolved in distilled water to make 0.0025-0.025 mol / L H 12 N6O6 platinum aqueous solution. Take 992.5ul H 12 The N6O6 platinum aqueous solution was added to 50 mL of H2O, and then 1 g of powdered indium zirconium oxide was immersed in the prepared H2O. 12 N6O6 platinum aqueous solution, stirred at room temperature for 3 hours. The obtained supported platinum indium zirconium oxide was dried in an oven at 80°C for 8-12 hours, and the solid was ground into powder after drying, and then the powder was calcined in a muffle furnace at 500°C for 3 hours to obtain an indium zirconium oxide supported single atom platinum catalyst with a platinum loading of 0.05%.
[0052] Example 4
[0053] A method for preparing an indium zirconium oxide-supported single-atom platinum catalyst comprises the following steps:
[0054] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.0375mol (NH4)2CO3 in 100mL H2O to form precipitant solution B; add these two solutions to a four-necked flask at a certain flow rate in a 70℃ water bath, and keep the pH of the solution at 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an 80℃ oven for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0055] H 12 N6O6 platinum powder was dissolved in distilled water to make 0.0025-0.025 mol / L H 12 N6O6 platinum aqueous solution. Take 1.985mL H 12 The N6O6 platinum aqueous solution was added to 50 mL of H2O, and then 1 g of powdered indium zirconium oxide was immersed in the prepared H2O. 12 N6O6 platinum aqueous solution, stirred at room temperature for 3 hours. The obtained supported platinum indium zirconium oxide was dried in an oven at 80°C for 8-12 hours, and the solid was ground into powder after drying, and then the powder was calcined in a muffle furnace at 500°C for 3 hours to obtain an indium zirconium oxide supported single atom platinum catalyst with a platinum loading of 0.1%.
[0056] Example 5
[0057] A method for preparing an indium zirconium oxide-supported single-atom platinum catalyst comprises the following steps:
[0058] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.0375mol (NH4)2CO3 in 100mL H2O to form precipitant solution B; add these two solutions to a four-necked flask at a certain flow rate in a 70℃ water bath, and keep the pH of the solution at 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an 80℃ oven for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0059] H 12 N6O6 platinum powder was dissolved in distilled water to make 0.0025-0.025 mol / L H 12 N6O6 platinum aqueous solution. Take 9.925mL H 12 The N6O6 platinum aqueous solution was added to 50 mL of H2O, and then 1 g of powdered indium zirconium oxide was immersed in the prepared H2O. 12N6O6 platinum aqueous solution, stirred at room temperature for 3 hours. The obtained platinum-loaded indium zirconium oxide was dried in an oven at 80°C for 8-12 hours, and the solid was ground into powder after drying, and then the powder was calcined in a muffle furnace at 500°C for 3 hours to obtain an indium zirconium oxide-loaded single-atom platinum catalyst with a platinum loading of 0.5%.
[0060] Example 6
[0061] A method for preparing an indium zirconium oxide-supported single-atom platinum catalyst comprises the following steps:
[0062] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.0375mol (NH4)2CO3 in 100mL H2O to form precipitant solution B; add these two solutions to a four-necked flask at a certain flow rate in a 70℃ water bath, and keep the pH of the solution at 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an 80℃ oven for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0063] Take 0.01985g H 12 N6O6 platinum powder was added to 50 mL of H2O, and then 1 g of powdered indium zirconium oxide was immersed in the prepared H2O. 12 N6O6 platinum aqueous solution, stirred at room temperature for 3 hours. The obtained platinum-loaded indium zirconium oxide was dried in an oven at 80°C for 8-12 hours, and the solid was ground into powder after drying, and then the powder was calcined in a muffle furnace at 500°C for 3 hours to obtain an indium zirconium oxide-loaded single-atom platinum catalyst with a platinum loading of 1%.
[0064] Example 7
[0065] A method for preparing an indium zirconium oxide-supported single-atom platinum catalyst comprises the following steps:
[0066] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.0375mol (NH4)2CO3 in 100mL H2O to form precipitant solution B; add these two solutions to a four-necked flask at a certain flow rate in a 70℃ water bath, and keep the pH of the solution at 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an 80℃ oven for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0067] Take 0.03969 g H12 N6O6 platinum powder was added to 50 mL of H2O, and then 1 g of powdered indium zirconium oxide was immersed in the prepared H2O. 12 N6O6 platinum aqueous solution, stirred at room temperature for 3 hours. The obtained platinum-loaded indium zirconium oxide was dried in an oven at 80°C for 8-12 hours, and the solid was ground into powder after drying, and then the powder was calcined in a muffle furnace at 500°C for 3 hours to obtain an indium zirconium oxide-loaded single-atom platinum catalyst with a platinum loading of 2%.
[0068] Example 8
[0069] A method for preparing an indium zirconium oxide-supported single-atom platinum catalyst comprises the following steps:
[0070] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.0375mol (NH4)2CO3 in 100mL H2O to form precipitant solution B; add these two solutions to a four-necked flask at a certain flow rate in a 70℃ water bath, and keep the pH of the solution at 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an 80℃ oven for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0071] Take 0.07938 g H 12 N6O6 platinum powder was added to 50 mL of H2O, and then 1 g of powdered indium zirconium oxide was immersed in the prepared H2O. 12 N6O6 platinum aqueous solution, stirred at room temperature for 3 hours. The obtained platinum-loaded indium zirconium oxide was dried in an oven at 80°C for 8-12 hours, and the solid was ground into powder after drying, and then the powder was calcined in a muffle furnace at 500°C for 3 hours to obtain an indium zirconium oxide-loaded single-atom platinum catalyst with a platinum loading of 4%.
[0072] Comparative Example 1
[0073] Indium zirconium oxide was prepared by the preparation method of Example 1.
[0074] Comparative Example 2
[0075] A method for preparing indium zirconium oxide comprises the following steps:
[0076] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.06mol urea in 100mL H2O to form precipitant solution B; add the two solutions to a four-necked flask at a certain flow rate in a water bath at 80℃, and keep the pH of the solution at 7-8; filter after aging for 2h, wash with deionized water 3 times and dry in an oven at 80℃ for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0077] The difference between Comparative Example 2 and Comparative Example 1 is that urea is used as the precipitant instead of the ammonium carbonate in Example 1.
[0078] Comparative Example 3
[0079] A method for preparing indium zirconium oxide comprises the following steps:
[0080] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.2mol Na2CO3 in 100mL H2O to form precipitant solution B; then add Na2CO3 solution dropwise to solution A under continuous stirring until the pH value of the solution in the beaker reaches 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an oven at 80℃ for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0081] The difference between Comparative Example 3 and Comparative Example 1 is that Na2CO3 is used as the precipitant instead of the ammonium carbonate in Example 1.
[0082] Comparative Example 4
[0083] A method for preparing indium zirconium oxide comprises the following steps:
[0084] Weigh 0.0125mol In(NO3)3·xH2O and 0.00625mol Zr(NO3)4·5H2O and dissolve them in 50mL H2O to obtain mixed salt solution A; dissolve 0.01875mol (NH4)2CO3 in 50mL H2O to form precipitant solution B; add solution B to solution A under stirring at 600rpm, then transfer the mixed solution to a 100mL polytetrafluoroethylene-lined hydrothermal synthesis reactor, place it in a blast drying oven for aging, the aging temperature is 70℃, and the aging time is 3h. After aging, filter and wash with deionized water for 3 times, and dry it in an oven at 80℃ for 12h. Calcinate in a muffle furnace at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e., indium zirconium oxide.
[0085] The difference between Comparative Example 4 and Comparative Example 1 is that the hydrothermal synthesis method is used instead of the precipitation method in Example 1 to prepare indium zirconium oxide.
[0086] Comparative Example 5
[0087] A method for preparing an indium zirconium oxide-supported single-atom platinum catalyst comprises the following steps:
[0088] Weigh 0.025mol In(NO3)3·xH2O and 0.0125mol Zr(NO3)4·5H2O and dissolve them in 100mL H2O to obtain mixed salt solution A; dissolve 0.0375mol (NH4)2CO3 in 100mL H2O to form precipitant solution B; add these two solutions to a four-necked flask at a certain flow rate in a 70℃ water bath, and keep the pH of the solution at 7-8; after aging for 2h, filter, wash with deionized water 3 times and dry in an 80℃ oven for 12h. Calcinate in air at 500℃ for 3h to obtain the catalyst oxidation state precursor, i.e. indium zirconium oxide.
[0089] H 12 N6O6 platinum powder was dissolved in distilled water to make 0.0025-0.025 mol / L H 12 N6O6 platinum aqueous solution. Take 198.5ul H 12 The N6O6 platinum aqueous solution was added to 50 mL of H2O, and then 1 g of powdered indium zirconium oxide was added to H2O at 80 °C and 600 rpm. 12 N6O6 platinum aqueous solution, then add 0.2g urea to the mixture and stir for 3h. The obtained loaded platinum metal oxide is dried in an oven at 80°C for 8-12h, and after drying, the solid is ground into powder, and then the powder is calcined in a muffle furnace at 500°C for 3h to obtain an indium zirconium oxide loaded single atom platinum catalyst with a platinum loading of 0.01%.
[0090] The difference between Comparative Example 5 and Example 1 is that the catalyst is prepared by using a precipitation method instead of the impregnation method in Example 1.
[0091] Performance Testing
[0092] 1. Microstructure
[0093] Figure 1 TEM image of the catalyst prepared in Example 1. Figure 1 It can be seen that the surface of indium zirconium oxide is evenly dispersed with nano-platinum atoms (see red circles).
[0094] 2.XRD
[0095] Figure 2The XRD patterns of the catalysts and indium zirconium oxides prepared in Example 1 and Comparative Example 1 (the abscissa 2θ represents the diffraction angle, and the ordinate Intensity represents the intensity of the diffraction peak) are shown in FIG. Figure 2 It can be seen that the catalyst prepared in Example 1 contains indium zirconium oxide and has no corresponding Pt XRD characteristic peak. This is because the lower Pt content and smaller Pt nanoparticles cannot be reflected in the diffraction peak.
[0096] 3. Catalytic performance of carbon dioxide hydrogenation
[0097] The catalysts prepared in Examples 1-8 and Comparative Examples 1-5 were respectively pressed into tablets at 15 MPa, ground, and screened to 40-80 meshes for evaluating their carbon dioxide hydrogenation catalytic performance.
[0098] 0.3 g of the selected catalysts were weighed and loaded into a reaction tube with an inner diameter of 8 mm. The catalysts were activated at 400 °C for 0.5 h in pure argon at normal pressure with a flow rate of 30 mL / min. The molar ratio of carbon dioxide to hydrogen was then switched to 3:1. The reaction was carried out at 3 MPa, 315 °C, and GHSV = 15000 cm 3 g -1 h -1 The catalyst evaluation results are shown in Table 1.
[0099] Table 1:
[0100]
[0101]
[0102] As can be seen from Table 1, in Examples 1-8 of the present invention, indium zirconium oxide is prepared by precipitation method using ammonium carbonate as a precipitant, and the catalyst prepared by impregnation method has better carbon dioxide conversion rate, methanol selectivity and space-time yield performance, achieving a carbon dioxide conversion rate of 11.00-14.20%, a methanol selectivity of 93.20-97.50%, and a methanol space-time yield of 0.521754-0.704541 gMeOH / g·h.
[0103] The catalyst of Comparative Example 1 is indium zirconium oxide. Compared with Example 1, due to the lack of single atomic platinum loading, its carbon dioxide conversion rate, methanol selectivity and space-time yield performance are all reduced.
[0104] The catalyst of Comparative Example 2-3 is indium zirconium oxide. Compared with Comparative Example 1, due to the use of other types of precipitants, the conversion rate of carbon dioxide and the space-time yield of methanol are both lower than those of Comparative Example 1.
[0105] Compared with Example 1, in Comparative Examples 4-5, the conversion rate of carbon dioxide, the selectivity of methanol and its space-time yield performance also decreased to varying degrees due to the use of hydrothermal synthesis in the preparation of indium zirconium oxide and precipitation method in the platinum loading process.
[0106] For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, without having to go through creative labor. Therefore, simple improvements made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the protection scope of the present invention. The above embodiments are preferred embodiments of the present invention, and all processes similar to the present invention and equivalent changes made should belong to the protection scope of the present invention.
Claims
1. A method for preparing a catalyst, characterized in that: The following steps are involved: (1) dissolving an indium source, a zirconium source, and a precipitant in water, adjusting the pH value, and subjecting the mixture to standing aging, filtering, washing, drying, and calcining to obtain indium zirconium oxide; the precipitant is ammonium carbonate; (2) Immersing the indium zirconium oxide in an aqueous solution of a platinum source, mixing, and drying; then grinding and calcining the dried solid to obtain the catalyst.
2. The method for preparing the catalyst according to claim 1, wherein The indium source includes indium nitrate tetrahydrate; and / or the zirconium source is selected from at least one of zirconium nitrate pentahydrate, zirconium oxynitrate pentahydrate, zirconium oxychloride, and zirconium oxide; and / or the molar ratio of the indium source to the zirconium source is (1-3):
1.
3. The method for preparing the catalyst according to claim 1, wherein The molar ratio of the zirconium source to the precipitant is 1:(2-4).
4. The method for preparing the catalyst according to claim 1, wherein In the aqueous solution of the platinum source, the solute is selected from at least one of platinum nitrate, chloroplatinic acid, and ammonium chloroplatinate; and / or the concentration of the aqueous solution of the platinum source is 0.0025-0.025 mol / L; and / or the mass volume ratio of the indium zirconium oxide to the aqueous solution of the platinum source is (1-2) g:1 mL.
5. The method for preparing the catalyst according to claim 1, wherein In step (1), the pH value is 7-8; and / or the calcination temperature condition is: calcination at 450-550° C. for 2-4 hours.
6. The method for preparing the catalyst according to claim 1, wherein In step (2), the calcination temperature condition is: calcination at 450-550° C. for 2-4 hours.
7. A catalyst, characterized in that Prepared by the preparation method according to any one of claims 1 to 6, the catalyst comprises indium zirconium oxide and single-atom platinum, and the single-atom platinum is uniformly loaded on the surface of the indium zirconium oxide.
8. The catalyst according to claim 7, characterized in that The loading amount of the single-atom platinum is 0.01-4 wt %.
9. A method for preparing methanol by hydrogenating carbon dioxide, characterized in that: The following steps are involved: The catalyst according to claim 7 or 8 is placed in a reactor, hydrogen and carbon dioxide are introduced, the temperature and pressure are increased, and the reaction is carried out to obtain the methanol.
10. The method for preparing methanol by hydrogenating carbon dioxide according to claim 9, characterized in that: The temperature is raised to 235-315°C; and / or the flow rate of the reaction gas is 6000-18000h -1 ; and / or, the pressure is increased to 1-4 MPa; and / or, the molar ratio of hydrogen to carbon dioxide is (1-5):1.